Effect of Post-Weld Heat Treatment on Creep Rupture Properties of ...
Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld...
Transcript of Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld...
![Page 1: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/1.jpg)
Procedia Engineering 86 ( 2014 ) 662 – 668
1877-7058 © 2014 The Authors. Published by Elsevier Ltd. This is an open access article under the CC BY-NC-ND license (http://creativecommons.org/licenses/by-nc-nd/3.0/).Peer-review under responsibility of the Indira Gandhi Centre for Atomic Researchdoi: 10.1016/j.proeng.2014.11.067
ScienceDirectAvailable online at www.sciencedirect.com
1st International Conference on Structural Integrity, ICONS-2014
Creep Crack Growth Behavior of a P91 Steel Weld
S. Venugopal*, G. Sasikala and Yatindra Kumar
Metallurgy & Materials Group, Indira Gandhi Centre for Atomic Research, Kalpakkam-603102, India *E-mail ID: [email protected]
Abstract
Modified 9Cr-1Mo steel (P91) weld joints operating at elevated temperatures are well known to be prone to premature failure due to cracking in the heat affected zone because of the gradients in microstructure, popularly referred to as Type IV cracking. A campaign was undertaken to study the creep crack growth behaviour of modified 9Cr-1Mo weld joints. Creep crack growth (CCG) tests were carried out on compact tension (CT) specimens machined from P91 weld joints prepared using multipass shielded manual metal arc welding procedure. Specimens with two notch locations have been employed, (i) within the weld metal, between the centreline and the fusion line and (ii) in the heat affected zone. Constant load CCG tests were carried out at different applied loads at 798 and 898 K. The C* - da/dt correlations (da/dt =A C*m) were established for both notch locations. At 898 K, a higher A (0.064) and lower m (0.533) for the case with notch placed in the HAZ, compared to those for the case of notch in the weld (0.0399 and 0.75 respectively) were observed indicating the higher creep crack growth in HAZ, confirming type IV cracking. The difference increases at lower C* levels which correspond to long term behaviour. Heavy creep damage was observed in the HAZ region even for the sample with notch in the weld, whereas the weld metal regions showed relatively less damage. As the crack grew, a change in its course to follow the HAZ region was observed. © 2014 The Authors. Published by Elsevier Ltd. Peer-review under responsibility of the Indira Gandhi Centre for Atomic Research.
Keywords: Creep crack growth, P91 steel, weld joint, heat affected zone
1. Introduction Creep crack growth (CCG) is a principal failure mechanism of components operating at elevated temperatures. The failure assessment codes and standards consider the CCG behaviour of materials, and more importantly those for the welds, in order to assess the reliability of such components. A modified 9Cr-1Mo steel (P91) has been chosen for the steam generator applications in the prototype fast breeder reactor (PFBR) designed by Indira Gandhi Centre for Atomic Research (IGCAR) and now in an advanced stage of construction at Kalpakkam. Type IV cracking in heat affected zone (HAZ) of weldments has long been recognised as a problem for advanced high Cr ferritic steels, see e.g. [1] for a review. Therefore, it is important to study initiation and growth of creep
© 2014 The Authors. Published by Elsevier Ltd. This is an open access article under the CC BY-NC-ND license (http://creativecommons.org/licenses/by-nc-nd/3.0/).Peer-review under responsibility of the Indira Gandhi Centre for Atomic Research
![Page 2: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/2.jpg)
663 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
voids and cracks in weldment. A study was initiated with the aim of characterizing the creep crack initiation and growth properties of different regions of P91 weld joints in the temperature range 798 to 898 K and also to characterize the effect of notch location on these properties. The preliminary results of this campaign are presented in this paper.
For materials creeping in the power law creep regime, the steady state stress field and strain rate distribution at any point (r, ) can be expressed using the fracture mechanics parameter C* as follows [2].
( )nrI
Cij
n
nij ,~*
11
000 θσ
εσσσ
+
= (1)
( )nrI
Cij
nn
n
cij ,~*
1
000 θε
εσεε
+
= (2)
where r is the radial distance from, and is the angle at the crack tip, n is the Norton exponent.
C* can be determined experimentally from the load line displacement rate ( Δ ) data as [3]
( )ηH
aWB
PC ⋅
−
Δ=* (3)
where P is the applied load, BN is the net thickness between side grooves, W is the width, a is the crack length, H and are specimen geometry dependent constants. For CT specimens, H = n/n+1 and = 2.2 according to ASTM E1457 [3]. The CCG rate ( a ) can be correlated to C* as
mCAdtda *⋅= (4)
The values of A and m characterise the CCG behaviour of the material.
2. Experimental The chemical composition of the P91 steel chosen for this study is given in Table 1. This was received in the form of plates of thickness 25 mm, in normalized (at 1323K for 30 min) and tempered (at 1053K for 75 min) condition. Welded joints were fabricated from the plates using multi-pass shielded metal arc welding (SMAW) process. Welding consumable used was of matching composition (Table 1) developed indigenously by IGCAR in collaboration with Indian industry.
Table 1: Chemical composition (in mass %) of the P91 steel and the weld
Element C Mn Si P S Cr Ni Mo V Nb N Al Ta Fe
P91 0.097 0.37 0.31 0.018 0.005 9.29 0.38 0.92 0.26 0.08 0.057 Bal
Weld 0.1 0.39 0.48 0.021 0.009 9.5 0.14 1.00 0.25 0.10 0.065 0.024 Bal.
Table 2: The details of preparation of weld pads
Consumable : P91 Electrode, Basic coated,
3.2 mm Number of passes : 50
Joint Design : Single V-groove Current : 90-110 A Process : Shielded Metal Arc Voltage : 20-24 V Preheat temp : 523 K Travel Speed : 2.75-3.0 mm/s Inter-pass temp. : 523 -573 K Heat input rate : 0.75-1.04 kJ/mm
![Page 3: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/3.jpg)
664 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
The weld pads were subjected to radiography to ensure the absence of any defects. Post-weld heat treatment of 1033K for 180 min was imparted to the weld pads. Compact tension (CT) type specimens of 20 mm thickness were fabricated from these pads. Two notch tip locations were used as schematically shown in Fig. 1; (A) within the weld metal about 2 mm from the fusion boundary (designated as type A specimen) and (ii) in the HAZ (designated as type B specimen). Fatigue pre-crack of ~ 5 mm was introduced at room temperature. The constant load CCG tests were completed for type A specimens in the load range 5 kN to 10 kN at 898 K, and for type B specimens, in the load range 20 to 30 kN at 798 K. Limited testing of type B specimens was carried out for comparison of CCG behaviour at the same stress intensity factor levels as type A at 898 K. Creep crack length was measured by D.C. electrical potential drop method. The load-line displacement was measured using single arm rod-and-tube type creep extensometer at the integral knife edges on the specimen.
3. Results and Discussion Typical plots of the variation of load line displacement and a with time are presented in Fig. 2 and 3 respectively for Type A specimens and Fig. 4 and 5 for Type B specimens. The data were analysed following the guidelines of ASTM E1457 [2]. Crack initiation time, t0.2, i.e., the time to attain 0.2 mm creep crack growth as a function of initial value of CCG parameter (C*) is presented in Fig. 6. It is observed that initiation time for both weld and HAZ follow the same scatter band. It should be noted that the tests on specimens with weld notch were carried out at 898 K, whereas those for HAZ notch were carried out at 798 K. However, considering the scatter typical of the initial CCG data, comparison of these should be done with caution. The crack growth rate (da/dt) as a function of C* for P91 weld joint specimens with the notch in weld and HAZ regions are presented in Fig. 7. In spite of the lower testing temperature for the specimen with HAZ notch, data for both notch locations fall in the same scatter band, indicating lower resistance to creep crack growth in HAZ.
Fig. 1: Schematic of the compact tension specimens indicating the notch location with reference to the weld deposit.
a
Base metal
Base metal
Weld metal Weld metal
b
Base metal
Base metal
![Page 4: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/4.jpg)
665 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
Fig. 4: Variation of creep displacement as a Fig. 5: Variation of crack length as a function of time for Type B specimens. function of time for Type B specimens.
0.0
1.0
2.0
3.0
4.0
5.0
6.0
7.0
0 500 1000 1500 2000
Time, h
Cra
ck e
xten
sion
, mm
30 kN25 kN20 kN
P91 weld-798 K Notch in HAZ
0.0
0.5
1.0
1.5
2.0
2.5
3.0
3.5
0 500 1000 1500 2000
Time, h
Dis
plac
emen
t, m
m 30 kN25 kN20 kN
P91 weld-798 K Notch in HAZ
0
0.5
1
1.5
2
2.5
3
3.5
4
4.5
5
0 1000 2000 3000 4000 5000 6000 7000
Time, h
Dis
plac
emen
t, m
m
P91Weld, 898 K, 5 kNNotch in the w eld region
0
1
2
3
4
5
6
0 50 100 150 200 250 300 35
Time, h
Dis
plac
em
ent,
mm
8 kN
10 kN
P91Weld, 898 KNotch in the w eld region
Fig. 2: Variation of creep displacement as a function of time for Type A specimens.
23
25
27
29
31
33
35
0 1000 2000 3000 4000 5000 6000 7000Time, h
Cra
ck le
ngth
, mm
P91Weld, 898 K, 5 kNNotch in the w eld region
P91Weld, 898 KNotch in the w eld region
23
24
25
26
27
28
29
30
31
32
0 50 100 150 200 250 300 350
Time, h
Cra
ck le
ng
th, m
m
8 kN
10 kN
Fig. 3: Variation of crack length as a function of time for Type A specimens.
![Page 5: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/5.jpg)
666 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
Comparison of the CCG Characteristics for the two Notch Location
For a clearer comparison, tests were conducted with the same initial value of stress intensity factor K for both types of specimens at the same temperature, namely, 898 K. The loads applied were chosen based on the initial crack lengths determined on the surface to yield a similar level of K. However, the initial crack lengths determined optically after the test were slightly different from those at the surface. Therefore, the type A specimens had a slightly higher initial K than type A specimen (19.8 and 17.9 MPa.m−1/2 respectively). The variations of displacement and crack growth with creep time are presented in Fig. 8.
1
10
100
1000
10000
0.01 0.1 1 10C*, kJ/m^2h
Initi
atio
n ti
me,
h
Notch in HAZ
Notch in weld
Fig. 6: Crack initiation time (t0.2) as a function of initial C* for the notch in weld and HAZ regions.
Fig. 7: The crack growth rate (da/dt) as a function of CCG parameter C* for P91 weld joint specimens with the notch in weld and HAZ regions.
Open symbols: Notch in Weld, 898 KSolid symbols: Notch in HAZ, 798 K
1.E-05
1.E-04
1.E-03
1.E-02
1.E-01
1.E+00
1.E+01
0.001 0.01 0.1 1 10 100
C*, kJ/m^2h
da/
dt,
mm
/h
![Page 6: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/6.jpg)
667 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
Even at a slightly higher K level, the crack growth rate in type A (weld) specimen was found to be consistently lower than that in type B (HAZ) specimen. The displacement rates were similar for both types in the steady state, but increased for the type B specimen towards the tertiary stage which set in earlier. The C* vs da/dt plots for the two types of specimen are shown in Fig. 9. It may be noted that the crack growth rate at the HAZ was higher than that in the weld metal at similar C* levels, especially at low C* levels indicative of long term effects.
Creep crack growth in the HAZ region is characterized by extensive creep void formation exclusively in the fine-grained heat-affected zone. This HAZ region is highly susceptible to creep damage accumulation due to the fine (average grain size of < 5 μm) equiaxed grain structure with no martensitic lath structure [4]. Extensive creep damage was observed in the HAZ region of type A specimens (Fig. 10) though this region is away from the highest stress concentration regions. In type B specimens, damage in this region is expected to be more extensive due to closer proximity to the notch tip and lead to a higher crack growth rate at longer durations corresponding to lower end of C* (Fig. 9).
The microstructural reasons for this may be explained as in the following. As mentioned earlier, the creep properties of weld deposits and the heat affected zones (HAZ), specifically for the class of 9Cr-1Mo steels, differ significantly from those of the base material since the welding process introduces very complex metallurgical and mechanical heterogeneities in to this region due to the solid state phase transformations, residual stresses and heat treatments [5]. The intercritical zone experiences peak temperature between Ac1 and Ac3 and only partial austenitization takes place here. The microstructure consists of fresh transformation products and re-tempered martensite. Also, coarse M23C6 carbides have been reported to be present in the intercritical zone in comparison to the parent metal P91 [6]. Creep deformation and damage evolution are significantly influenced by the presence of fine precipitates and second phase particles, in addition to the solid solution hardening. Various types of carbides and carbonitride such as M23C6, M6C, M3C, M7C3, M5C2, M2X, MX etc and phases (Laves) have been reported to
0
0.5
1
1.5
2
2.5
3
3.5
0 100 200 300 400
Time, h
Dis
plac
emen
t, m
mHAZ
weld
23
25
27
29
31
33
0 100 200 300 400
Time, h
Cra
ck le
ngth
, mm
HAZ
weld
Fig. 8: Variations of displacement and crack length as a function of time.
0.1 1 101E-3
0.01
0.1
1
da/dt = 0.064C*0.53
da/dt = 0.0399C*0.75
P91 weld joint898 K
Notch in HAZ Notch in Weld
da/d
t, m
m.h
−1
C*, kJ.m−2.h−1
Fig. 9: The C* vs da/dt plots for the two types of specimens at similar initial K levels.
Fig. 10: Extensive creep damage observed in the heat affected zone of the weld joint.
![Page 7: Creep Crack Growth Behavior of a P91 Steel Weld · Creep Crack Growth Behavior of a P91 Steel Weld S. Venugopal*, G. Sasikala and Yatindra Kumar ... shielded manual metal arc welding](https://reader031.fdocuments.net/reader031/viewer/2022022513/5aefe41a7f8b9aa9168d360e/html5/thumbnails/7.jpg)
668 S. Venugopal et al. / Procedia Engineering 86 ( 2014 ) 662 – 668
be present in the steel of this class [7]: and Laves phases. Grain boundary sliding and grain boundary migration which accompany the creep deformation are also influenced by the precipitates. Damage nucleation and growth rates are enhanced by the stress concentration near these precipitates [8]. Also, coarsening of M23C6 or Laves phase (Fe,Cr)2Mo due to long term thermal exposure leads to a decrease in the creep resistance [9] of the HAZ. Formation of Z phase, Cr(V,Nb)N, at the expense of VN-precipitates is another factor that leads to a long term degradation effect.
Conclusions
The creep crack growth behavior of P91 weld joint has been characterized using the fracture mechanics parameter C* for two different notch locations, and da/dt-C* correlations were established. Crack initiation time was found to be a function of initial C* for both location and for HAZ notch at 798 K was similar to that for weld notch at 898K. The CCG rates were found to be higher in the HAZ region, especially for low C* levels as indicated by a higher A value in the da/dt-C* correlation.
References
1. Francis J. A., Mazur W., and Bhadeshia H. K. D. H., Type IV cracking in ferritic power plant steels, Materials Science and Technology, 2006 VOL 22 NO 12, 1387.
2. Webster GA, Ainsworh RA. High temperature component life assessment, London, Chapman & Hall; 1994.
3. ASTM E1457-07, Standard Test Method for Measurement of Creep Crack Growth Times in Metals. ASTM International, 100 Barr Harbor Dr., P.O. box C700 West Conshohocken, Pennsylvania 19428-2959, United States, 2007.
4. Peter Mayr, Stefan Mitsche, Horst Cerjak, Samuel M. Allen, The Impact of Weld Metal Creep Strength on the Overall Creep Strength of 9% Cr Steel Weldments, Trans ASME Journal of Engineering Materials and Technology, Vol. 133, 2011,021011-1 to 7
5. Bhadeshia, H. K. D. H., ISIJ International, 41, 2001, p. 626. 6. Laha K.,Chandravathi K. S., Bhanu Sankara Rao K., Mannan S. L., Sastry D. H, Trans. Indian Inst. Met.,
53, 2000, p. 217. 7. Hald, J., In: Advanced Creep Data for Plant Design & Life Extension (Proc. of Int Seminar),. Praha,
SVÚM 2003, p. 58. 8. Ashby M. F.,Gandhi C., Taplin D. M. R., Acta Met., 27, 1979, p. 699. 9. Panait C, Bendick W, Fuchsmann A, Gourgues-Lorenzon A-F, Besson J. Study of the microstructure of the
grade P91 steel after more than 100,000h of creep exposure at 600°C, Inter. J. Press. Vess. Pip. 87, 326-335.