2. Injection Moulding.ppt
Transcript of 2. Injection Moulding.ppt
![Page 1: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/1.jpg)
INJECTION MOULDING
![Page 2: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/2.jpg)
Historical Background
• A single-action hydraulic injection machine was designed in the U.S.A. in 1870 by Hyatt
• Heating-cylinder design was first recognised in a patent issued to Adam Gastron in 1932.
• Large-scale development of injection moulding machinery design towards the machines we know today did not occur until the 1950's in Germany
![Page 3: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/3.jpg)
Injection Moulding Process – Over View
Solid Wide neck, Flat Product is made like bucket, cabinets, Automobile & Industrial parts etc…. by injecting molten thermoplastic material in to a closed mould which is relatively cool.
![Page 4: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/4.jpg)
Type of Injection Moulding Machine
• Hand Injection Moulding M/C
• Plunger type Injection Moulding M/C
• Reciprocating Screw Type Injection Moulding M/C
![Page 5: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/5.jpg)
Hand Injection Moulding Machine
vertical machine consists of Barrel, Plunger, Band Heaters along with energy regulator, Rack & Pinion system for Injecting the material by the plunger, a torpedo and nozzle.
![Page 6: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/6.jpg)
Plunger Type Injection Moulding Machine
Vertical & Horizontal Plunger Type Injection Moulding Machine
![Page 7: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/7.jpg)
The Reciprocating Screw
• The feeding zone • The compressing (or transition) zone • The metering zone
![Page 8: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/8.jpg)
Machine components
![Page 9: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/9.jpg)
The Injection Process
• Plasticises the material by reciprocating Screw.• Injects the molten material to a closed mould
– via a channel system of gates and runners.
• Cools the Mould.• Refills the material for the next cycle.• Ejects the Product.• Closes the Mould for further cycle.
![Page 10: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/10.jpg)
Injection Moulded Items
![Page 11: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/11.jpg)
Injection Moulded Items
![Page 12: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/12.jpg)
Injection Moulded Items
![Page 13: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/13.jpg)
Advantages of Injection Moulding Process
• Parts can be produced at high production rates.• Large volume production is possible.• Relatively low labour cost per unit is obtainable.• Process is highly susceptible to automation.• Parts require little or no finishing.• Many different surfaces, colours, and finishes are
available.• Good decoration is possible.• For many shapes this process is the most economical way
to fabricate.• Process permits the manufacture of very small parts which
are almost impossible to fabricate in quantities by other methods.
![Page 14: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/14.jpg)
Advantages of Injection Moulding Process
• Minimal scrap loss result as runners, gates, and rejects can be reground and reused.
• Same items can be moulded in different materials, without changing the machine or mould in some cases.
• Close dimensional tolerances can be maintained.• Parts can be moulded with metallic and non-metallic
inserts.• Parts can be moulded in a combination of plastic and
such fillers as glass, asbestos, talc and carbon.• The inherent properties of the material give many
advantages such as high strength-weight rates, corrosion resistance, strength and clarity.
![Page 15: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/15.jpg)
Limitations of Injection Moulding • Intense industry competition often results in low profit
margins.
• Mould costs are high.
• Moulding machinery and auxiliary equipment costs are high.
• Lack of knowledge about the fundamentals of the process causes problems.
• Lack of knowledge about the long term properties of the materials may result in long-term failures.
![Page 16: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/16.jpg)
Machine operation sequence The mould closes and the screw begins moving forward for injection.
The cavity fills as the reciprocating screw moves forward, as a plunger.
![Page 17: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/17.jpg)
Machine operation sequence The cavity is packed as the screw continuously moves forward.
The cavity cools as the gate freezes off and the screw begins to retract to plasticize material for the next shot.
![Page 18: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/18.jpg)
Machine operation sequence
The mould opens for part ejection
The mould closes and the next cycle begins
![Page 19: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/19.jpg)
Injection Mould
![Page 20: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/20.jpg)
Mould system A typical (three-plate) moulding system
![Page 21: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/21.jpg)
A two-plate mould. A three-plate mould.
The moulded system includes a delivery system and moulded parts.
![Page 22: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/22.jpg)
Screw Used in Injection Moulding Machines
The screw has three zones with a ring-plunger assembly. The Feed Zone, where the plastic first enters the screw and is conveyed along a constant root diameter; the Transition Zone, where the plastic is conveyed, compressed and melted along a root diameter that increases with a constant taper; and the Metering Zone, where the melting of the plastic is completed and the melt is conveyed forward along a constant root diameter reaching a temperature and viscosity to form parts.
![Page 23: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/23.jpg)
L/D RATIO
• The L/D ratio is the ratio of the flighted length (Effective Length) of the screw to its outside diameter.
• Most injection screws use a 20:1 L/D ratio. But it may range from 18:1 to 24:1
• In the case of Thermoset it may range from 12:1 to 16:1.
![Page 24: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/24.jpg)
High L/D Ratio results the following ….
• More shear heat can be uniformly generated in the plastic without degradation;
• Greater the opportunity for mixing, resulting in a better homogeneity of the melt.
• Greater the residence time of the plastic in the barrel possibly permitting faster cycles of larger shots.
![Page 25: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/25.jpg)
COMPRESSION RATIO (CR) • The ratio of the first flight depth of feed zone to the last
flight depth of meter zone , Or,• First Channel Volume of feed zone to last channel
volume of metering zone,
• Typically ranges from 1.5:1 to 4.5:1 for most thermoplastic materials.
• Most injection screws classified as general purpose have a compression ratio of 2.5:1 to 3.0:1.
• Thermo set screws have a 1:1 ratio.
![Page 26: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/26.jpg)
Higher the CR results the following ….
• Greater shear heat imparted to the resin
• Greater heat uniformity of the melt
• High Potential for creating stresses in some resins
• High energy consumption
![Page 27: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/27.jpg)
Back Pressure (Kg/Cm2 or bar) Back pressure is the amount of pressure
exerted by the material ahead of the screw, as the screw is pushed back in preparation for the next shot.
Effect of Back Pressure • More Homogeneous Mix• Proper Melting• More compact• Sometime leads degradation
![Page 28: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/28.jpg)
Injection Speed (cm/Sec) The injection speed is the forward
speed of the screw during its injection operation per unit time.
Effect of Injection Speed• Easy Injection of Material
• Avoid Short-Shot
• Some times leads more orientation & burn marks
![Page 29: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/29.jpg)
Screw Rotation Speed
The screw rotation speed (RPM) is the rate at which the plasticizing screw rotates.
The faster the screw rotation result the following ..
• Faster the material is compressed by the screw flights
• Increasing the amount of shear heating
• Low residence time, some less melting
![Page 30: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/30.jpg)
Cushion The cushion is the difference in the final forward position
of the screw and its maximum allowable forward position.
• More Cushion results more residence time, some time degrades.
• If the screw were allowed to travel its full stroke and stop mechanically against the nozzle, the cushion would be zero.
• With zero Cushion no hold on works.
• Typically a cushion of 3 to 6 mm is used.
![Page 31: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/31.jpg)
Materials for Injection Moulding • Acrylonitrile butadiene styrene (ABS) • Acetal • Acrylic • Polycarbonate (PC) • Polyester • Polyethylene • Fluoroplastic • Polyimide • Nylon • Polyphenylene oxide • Polypropylene (PP) ** • Polystyrene (PS) • Polysulphone • Polyvinyl chloride (PVC)
![Page 32: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/32.jpg)
![Page 33: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/33.jpg)
Molecules lie in a definite fashion or regular arrangement
![Page 34: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/34.jpg)
![Page 35: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/35.jpg)
Molecules fall in Crystalline & amorphous pattern
![Page 36: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/36.jpg)
Amorphous Polymer has
![Page 37: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/37.jpg)
![Page 38: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/38.jpg)
While flowing in the channel or cavity of the Mould. As the melt touches the surface of the mould its viscosity increases because of lowering of melt temperature, So it slides on the Surface and the Molecules gets oriented
![Page 39: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/39.jpg)
![Page 40: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/40.jpg)
![Page 41: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/41.jpg)
![Page 42: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/42.jpg)
Non Newtonian Plastics
![Page 43: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/43.jpg)
Non Newtonian Plastics
![Page 44: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/44.jpg)
![Page 45: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/45.jpg)
Newtonian Plastic
![Page 46: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/46.jpg)
![Page 47: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/47.jpg)
![Page 48: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/48.jpg)
![Page 49: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/49.jpg)
![Page 50: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/50.jpg)
![Page 51: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/51.jpg)
Broad Molecular weight Distribution shows broad Melting Points
![Page 52: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/52.jpg)
Narrow Molecular weight Distribution shows sharp Melting Points
![Page 53: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/53.jpg)
Plastic Product Properties can change 10% or more by changing Process Conditions
![Page 54: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/54.jpg)
![Page 55: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/55.jpg)
![Page 56: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/56.jpg)
![Page 57: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/57.jpg)
![Page 58: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/58.jpg)
![Page 59: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/59.jpg)
![Page 60: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/60.jpg)
![Page 61: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/61.jpg)
![Page 62: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/62.jpg)
![Page 63: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/63.jpg)
![Page 64: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/64.jpg)
During Refilling
![Page 65: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/65.jpg)
During Injection
![Page 66: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/66.jpg)
![Page 67: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/67.jpg)
![Page 68: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/68.jpg)
![Page 69: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/69.jpg)
Additive Function Examples
Filler increase bulk density calcium carbonate, talc, limestone
Plasticizer improve processability, reduce product brittleness
phthalate esters, phosphate esters
Antioxidant prevent polymer oxidation phenols, aromatic amines
Colorant provide desired part application color
oil-soluble dyes, organic pigments
Flame retardant
reduce polymer flammability antimony trioxide
Stabilizer stabilize polymer against heat or UV light
carbon black, hydroxybenzophenone
Reinforcement improve strength E-glass, S-glass, carbon, Kevlar fibers
![Page 70: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/70.jpg)
TOGGLE TYPE CLAMPING
• A toggle is mechanically device to amplify force. • In a moulding machine, which consists of two bars
joined, together end to end with a pivot .• The end of one bar is attached to a stationary platen,
and the other end of a second bar is attached to the movable platen.
• When the mould is open, the toggle is in the shape of a V.
• When pressure is applied to the pivot, the two bars form a straight line.
![Page 71: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/71.jpg)
TOGGLE TYPE CLAMPING
![Page 72: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/72.jpg)
ADVANTAGE
• Low cost and lower horsepower needed to run.• Positive clamp of the mould
DISADVANTAGE
• Do not read the clamp force.• Clamping is more difficult.• Higher maintenance as lubricant is provided.
TOGGLE TYPE CLAMPING
![Page 73: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/73.jpg)
HYDRAULIC CLAMPING
• A clamping unit actuated by hydraulic cylinder, which is directly connected to the moving, closed the mould. In this case ram of hydraulic system is attached to moving platen. There are two halves in hydraulic cylinder, which is actually inlet and outlet of oil.
• When oil goes to the cylinder with pressure oil pushes the ram to forward direction by which moving platen moves and mould closed and when oil comes from the cylinder the ram come back and mould is open.
![Page 74: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/74.jpg)
HYDRAULIC CLAMPING
![Page 75: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/75.jpg)
ADVANTAGE
• Clamp speed easily controlled and stopped at any point.• Direct a read out of clamp force.• Easy adjustment of clamped force and easy mould set
up.• Low maintenance as part is self lubricated.
DISADVANTAGE
• It is higher cost and more expensive than toggle system.
• None positive clamp.
HYDRAULIC CLAMPING
![Page 76: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/76.jpg)
TIE-BAR LESS CLAMPING• Tie-Bar less clamping system is basically Hydraulic
clamping system without any tie bar.
• The platen is moved on a rail system.
• The main advantage of this system there is no limitation of mould platen size.
• As there is no tie bar so the mould dimension is not so important.
• Also mounting of the mould is easy and it is very useful when products eject from the mould is manual.
![Page 77: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/77.jpg)
TIE-BAR LESS CLAMPING
![Page 78: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/78.jpg)
TIE-BAR LESS CLAMPING• Much larger mould mounting area. • Larger stroke compared to the toggle type machines. • Full machine capacity can be utilised. • Smaller machines can mould larger components. • Saves floor space. • Saves electrical energy because of reduction in the size of machine. • Has the capacity to reduce weight of the moulded component because tie-
bar stretching is not there. • Machine becomes very flexible for future modification. • Easy access to mould cavity's because of the absence of the tie bars. • Robotic arm movement becomes easy. • Fewer moving parts so lesser wear and tear so longer life for machines. • Lower lubrication required. • Removal of mould plates much simple. • Greater stability.
![Page 79: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/79.jpg)
Theoretical Calculation
![Page 80: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/80.jpg)
Example 1: POM has an S.G. of 1.42. It is to be moulded in an Injection Moulding Machine with a shot weight of 80 gms (in PS).
This machine has a shot weight of 80 x 1.42 / 1.05 = 108.19 gms of POM.
Example 2: PP has an S.G. of 0.90. It is to be moulded in an Injection Moulding Machine with a shot weight of 80 gms (in PS).
This machine has a shot weight of 80 x 0.90 / 1.05 = 68.57 gms of PP.
![Page 81: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/81.jpg)
Example 3: Figurines made of UPVC (S.G. 1.38) with a combined weight of figurine plus runners of 40 gms. are to be moulded. What size of machine is sufficient?
Shot weight in terms of PS = 40 x 1.05/1.38 = 30.43 gms.
Using the 85% guide line, the machine shot weight needed = 30.43/0.85 =35.80 gms.
Example 4: The same figurine in example 3 is to be moulded in a big machine. What is the biggest machine that could be used?
Using the 35% rule, the biggest machine that could be used has a shot weight = 30.43/0.35 = 86.94 gms.
![Page 82: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/82.jpg)
Projected area is calculated by multiplying length times width.
Determining Projected Area
![Page 83: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/83.jpg)
Projected Area = Length x Width
and multiplying that area by a clamp factor of between 2 and 8. Most commonly factor 5 is used.
Clamp Force = Projected Area x 5
For every inch of depth the clamp force must be increased by 10%.
Determining Clamping Force (Tonnes)
![Page 84: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/84.jpg)
Example 5: What is the residence time of UPVC (S.G. 1.38) in a machine with screw diameter of 55 mm, injection stroke of 250 mm, shot weight (PS) of 567 g, and a cycle time of 10 s moulding shots weighing 260 g?
Volume of melt in the barrel is estimated to be two times the injection volume = 2 * 3.1416 * 5.5 * 5.5 * 25 / 4 = 1188 cm3 Barrel residence time = 1188 * 1.38 * 10 / 260 = 63 s
Example 6: A GPPS cup of diameter 79 mm is to be moulded. The cup is 0.6 mm at its thinnest section. Find a conservative clamping force which would be sufficient.
The projected area of the cup (and runner) is 3.1416 * 7.92 / 4 = 49 cm2.
This cup belongs to the thin wall domain. The conservative clamping force is 0.62 * 49 = 30.4 tonnes.
![Page 85: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/85.jpg)
Example 7: The same GPPS cup has a flow path length of 104 mm. Find a more accurate clamping force needed.
Flow path to thickness ratio (L/T Ratio) = 104 / 0.6 = 173. From Figure 2, at 0.6 mm wall thickness, the cavity pressure is 550 bar. 1 bar = 1.02 kg/cm2. The clamping force = 550 * 1.02 * 49 = 27,500 kg = 27.5 tonnes.
The above calculation has not accounted for viscosity. It turns out to be still correct as the viscosity factor for GPPS is 1.0.
Example 8: The same cup as in the above example is to be made out of ABS. Find the clamping force needed.
Using the viscosity factor of 1.5, the clamping force needed = 1.5 * 27.5 tonnes = 41.3 tonnes.
![Page 86: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/86.jpg)
Plastic flow
(a)Simple shear flow. (b)Simple extensional flow.
(c) Shear flow in cavity filling. (d) Extensional flow in cavity filling.
![Page 87: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/87.jpg)
where
![Page 88: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/88.jpg)
When Plastics flow in the cavity, the pressure decreases along the delivery system and the cavity
![Page 89: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/89.jpg)
Injection pressure as a function of melt viscosity, flow length, volumetric flow rate, and part thickness
![Page 90: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/90.jpg)
Setting Machine Process Conditions 1 Set the melt temperature
2 Set the mold temperature
3 Set the switch-over position
4 Set the screw rotation speed
5 Set the back pressure
6 Set the injection pressure to the machine maximum
7 Set the holding pressure at 0 MPa
8 Set the injection velocity to the machine maximum
9 Set the holding time
10 Set ample remaining cooling time
![Page 91: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/91.jpg)
Setting Machine Process Conditions
11 Set the mold open time
12 Mold a short-shot series by increasing injection volume
13 Switch to automatic operation
14 Set the mold opening stroke
15 Set the ejector stroke, start position, and velocity
16 Set the injection volume to 99% mold filled
17 Increase the holding pressure in steps
18 Minimize the holding time
19 Minimize the remaining cooling time
![Page 92: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/92.jpg)
Basic Process Factors in Injection Moulding
• Material Parameters – Amorphous, Semicrystalline, Blends and Filled Systems – Pressure-Volume-Temperature (PVT) Behaviour – Viscosity
• Geometry Parameters – Wall Thickness of Part – Number of Gates – Gate Location – Gate Thickness and Area – Type of Gates: Manually or Automatically Trimmed – Constraints from Ribs, Bosses and Inserts
• Manufacturing Parameters – Fill Time – Packing Pressure Level – Mold Temperature – Melt Temperature
![Page 93: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/93.jpg)
Residual stress
The development of residual flow stresses due to frozen-in molecular orientation during the filling and packing stages. (1) High cooling, shear, and orientation zone (2) Low cooling, shear, and orientation zone
![Page 94: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/94.jpg)
![Page 95: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/95.jpg)
Process Controls Injection Moulding cycle can be broken down into four
phases: • Fill, • Pack, • Hold, and • Cooling/plastication
These phases can be controlled by following variables:
• Injection Speed, • Plastic Temperature, • Plastic Pressure, • Cooling Temperature and Time.
![Page 96: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/96.jpg)
![Page 97: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/97.jpg)
![Page 98: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/98.jpg)
Cycle time in injection moulding
![Page 99: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/99.jpg)
![Page 100: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/100.jpg)
Post Moulding Operation
• Heat inserting
• Chrome Plating
• In Mould Insert Moulding
• Post Mould Inserting
• Drilling
• Polishing
• Assembly
![Page 101: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/101.jpg)
Secondary operations
• Bonding
• Welding
• Inserting
• Staking
• Swaging
• Assembling with fasteners
![Page 102: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/102.jpg)
Secondary operations
• Appliqué: a surface covering applied by heat and pressure
• Printing: a process of making a mark or impression onto a substrate for decorative or informational purposes.
• Painting • Hard coating • Metallizing/shielding • Surface treatment • Annealing • Machining
![Page 103: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/103.jpg)
Benefits of Post Moulding Operations
• Reduced costs – by carrying out post moulding operations in house, and utilising lean manufacturing tools, we can greatly reduce component costs and the complexity of work that our customers would ordinarily undertake.
• High level of quality – performing post-moulding operations on products helps ensure that a high level of quality is maintained. By checking parts from the moment they leave a press, to final assembly, quality levels can be maintained and ensure that components are only assembled to the highest standards.
• Reduction of Customer’s stock holding – Assembly of components will reduce the cost of customers stock holding due to delivery of an assembly rather than a range of components.
• Reduced production times – post moulding operations mean there is very little time between the production of components and their assembly. This means that a great deal of time can be saved when components would normally be transported, or stored, in between moulding and assembly operations.
![Page 104: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/104.jpg)
Heat inserting is the addition of inserts into a part increases the functionality of a part by which components can be assembled.
![Page 105: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/105.jpg)
Benefits of Heat Inserting
• Increased functionality – by adding inserts to mouldings the part can more easily be used for its designed purpose. For example by adding threaded inserts parts can be easily be screwed to their fixings or other parts, increasing their functionality.
• Low part degradation – the process of heat inserting means that the heating/melting of the part is very localised to where the insert will be pressed in. this means that parts do not suffer warping, or any other distortion effects, due to being heated again.
• High level of quality – due to the known challenges with heat inserting extra measures are taken to ensure the processes is repeated to as high a level as possible, meaning part quality is kept very high.
![Page 106: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/106.jpg)
Chrome Plating
Due to the chrome plating process requiring the part to be electrically conductive, a series of steps are required before the chrome can be deposited onto the surface of the product.
![Page 107: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/107.jpg)
Benefits of Chrome Plating• Metal finish - Metal finishes can be very popular and, by
coating plastics, advantage can be taken of characteristics from both materials.
• Wear resistant – as chrome is a metal rather than a plastic its wear resistance properties are much greater than those of the plastic it covers. This means for applications where a part might be handled repeatedly, such as a shower handset, a chrome finish is likely to wear better than its plastic counterpart.
• Electrically conductive parts – by chrome or nickel plating a part it is possible to give a plastic component the ability to conduct electricity. This gives the advantage of being able to create electrical components that are light weight and less costly to produce than completely metal parts.
• Attractive mouldings – by applying chrome finish to mouldings a
![Page 108: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/108.jpg)
In Mould Insert Moulding
In mould insert moulding is the process by which a metal, or preformed plastic, insert is incorporated in to the component during the moulding stage.
![Page 109: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/109.jpg)
Benefits Of In Mould Insert Moulding• Reduced post-moulding operations – With in mould insert moulding the
need for post moulding operations is greatly reduced. This helps with ease of assembly and reduces the labour necessary for products.
• Increased part consistency – Insert Moulding has major benefits in the consistency of parts produced. As the inserts are placed in the same locations in tools for every cycle each of the mouldings produced will be exactly the same. This helps reduce costs, as rejected parts will be kept to a minimum.
• Ease of assembly – Due to inserts being incorporated into parts during the moulding stage this eases the assembly of the part. Instead of having to place fittings to attach parts fittings can be incorporated during the moulding stage so that parts can be simply clipped together.
• Reduced production time – when vertical moulding machines, that are equipped with a rotary table, are used for production there is the opportunity to have two halves of the lower part of the tool. This means that production is almost constant with mouldings being formed at the same time as fresh inserts are being loaded into the second half of the tool. This lowers overall production times and can also reduce the amount of labour needed.
![Page 110: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/110.jpg)
Post Mould Inserting
Post mould inserting is the process by which a metal, or preformed plastic, insert is incorporated into a moulding by means of a secondary process once the component has already been moulded.
![Page 111: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/111.jpg)
Benefits of Post Mould Inserting
• Ease of assembly – by adding inserts to a moulding the ease by which it can be assembled is greatly increased. Inserts such as clips or screw bolts can be incorporated into mouldings which greatly assist assembly operations and subsequent product performance.
• Increased part functionality – besides adding inserts to aid assembly inserts that improve a parts functionality can also be used. For example, terminal fittings for wires, or seals to make parts watertight.
• Increased component value – any second operation carried out on a part will add value to it. By adding inserts to help assembly or increase functionality, product value will be raised. This helps to compensate for the extra time involved in second operations and ensure products remain cost effective.
• Good part consistency – to carry out post mould inserting jigs are used to hold mouldings while they are inserted. This means that the repeatability of the operation is very good and all parts inserted will be of the same quality.
![Page 112: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/112.jpg)
Drilling
The drilling of parts is used to remove any unnecessary polymer that may have been necessary in the moulding process. By removing this extra material in house it means a ready-to-assemble moulding can be provided to the customer, or the part can be assembled with other mouldings.
![Page 113: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/113.jpg)
Polishing
For products that have a high quality gloss finish a post moulding polishing operation is often a useful extra process. Even though the finish produced by the moulding tool may be of a very high quality, a polishing operation to remove any dust from the product before final packaging gives a part the high gloss finish that will have been specified.. Polishing operations are carried out on a soft-polishing wheel with high quality wax to ensure that a part is polished to a perfect finish without leaving any marks.
![Page 114: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/114.jpg)
Assembly
For products that require assembly we are able to carry out this operation in our assembly facility. We can demonstrate examples of assemblies where we mould all the separate components in house and assemble the parts either as a whole in the assembly facility or as a step by step process on the press as each part is produced. By carrying out assembly in house we can reduce costs for our customers while still producing products to a high standard.
![Page 115: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/115.jpg)
Faults & Remedies
![Page 116: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/116.jpg)
Sink Marks
Depression in a moulded part caused by shrinking or collapsing of the resin
during cooling.
![Page 117: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/117.jpg)
Sink Marks - Problems
• Resin feed inadequate• Improper mould design.• Parts cool too rapidly• Rib section in part too wide.• Temperature of mould
surface opposite rib too hot.• Entrapped gas.• Nozzle too restrictive, • land length too long.
• Pressure too low.• Mould temperature too low
or high• Stock temperature too high• Gate too small• Improper gate location• Nozzle and metering zone
temperatures too high.• Excessive cooling time in
mould• Unbalanced flow pattern.• Bad check valve.
![Page 118: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/118.jpg)
Jetting
Turbulence in the resin melt flow caused by undersized gate, abrupt change in cavity volume, or too high injection
pressure.
![Page 119: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/119.jpg)
Jetting - Problems
• Excessive injection speed.• Melt temperature too high.• Melt temperature too low.• mould Temperature too low.• Nozzle opening too small.• Gate and length too long.• Sprue, runner, and/or gate size too small.• Nozzle heating band malfunction.• Inefficient gate location.
![Page 120: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/120.jpg)
Splay Marks (Silver Streaking, Splash Marks)
Marks or droplet type imperfections formed on the surface of a finished
part.
![Page 121: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/121.jpg)
Splay Marks (Silver Streaking, Splash Marks) - Problems
• Obstruction in nozzle.• Screw rpm too high.• Back pressure too low.• Melt temperature too
high.• Nozzle too hot.• Nozzle too small.• Gates too small.• Sprue too small.• Insufficient venting.
• Burr in runner or gate.• Cracked mould.• Trapped volatiles.• Excessive moisture.• Resin contaminated.• mould cavity
contamination.• Excessive shot size.
![Page 122: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/122.jpg)
Blush
Discoloration generally appearing at gates, around inserts, or other obstructions along the flow path. Usually indicates
weak points.
![Page 123: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/123.jpg)
Blush - Problems
• mould temperature too cold• Injection fill speed too fast• Melt stock temperature too high or too low.• Improper gate location• Sprue and nozzle diameter too small.• Nozzle temperature too low.• Insufficient cold slug well.• Sharp Corners in gate area• Resin excessively moist.• Inadequate injection pressure.
![Page 124: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/124.jpg)
Burn Marks
Black marks or scorch marks on surface moulded part; usually on the side of the
part opposite the gate or in a deep cavity.
![Page 125: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/125.jpg)
Burn Marks - Problems• Excessive Injection speed• Excessive injection
pressure.• Inefficient mould
temperature.• Excessive amount of
volatiles due to improper Venting.
• Improper gate location• Front zone temperature too
high. • Screw speed too high.• Excessive back pressure.• Compression ratio of screw
too high.
• Faulty temperature controllers.
• Frictional burring--gates too small
• Dead material hung up on screw or nozzle.
• Melt stock temperature too high or too low.
• Nozzle diameter too small• Over-heated heater band• Incorrect screw rpm.
![Page 126: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/126.jpg)
Poor Weld Lines (Knit Lines)
Inability of two melt fronts to knit together in a homogeneous fashion during the
moulding process, resulting in weak areas in the part of varying severity.
![Page 127: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/127.jpg)
Poor Weld Lines - Problems
• Material too cold.• Injection speed too slow• Entrapment of air at weld
line.• Improper mould design.• Contamination of poorly
dispersed pigments.• Core shifting.• mould temperature to low.• Injection speed too slow.• Melt stock temperature to
low.• Injection pressure too low.
• Insufficient mould venting• Cylinder temperature too
low.• Injection back pressure too
low.• Nozzle diameter too small.• Excessive screw flights in
metering zone.• Improper gate locations
and/or size.• Distance from gate
excessive.• Ineffective flow pattern.• mould release agent (brittle
weld lines).• Inadequate flow.
![Page 128: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/128.jpg)
Voids (Bubbles)
An unfilled space of such size that it scatters radiant energy such as light.
![Page 129: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/129.jpg)
Voids - Problems
• Injection pressure too low• Packing time too short• Insufficient feed of material• mould temperature too low.• Injection speed too high• Excessive cushion• At the side of a rib; rib too thick.• Runners or gate too small or badly
positioned.
![Page 130: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/130.jpg)
Delamination (Skinning)
Surface of the finished part separates or appears to be composed of layer of
solidified resin. Strata or fish scale type appearance where the layers may be
separated.
![Page 131: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/131.jpg)
Delamination - Problems
• Contamination of resin by additives or other foreign materials.
• Resin temperature too low.• Non-uniformity of resin temperature.• Wrong mould temperature.• Excessive material moisture.• Inadequate injection speed.• Sharp corners at gate.• Incompatible polymers.
![Page 132: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/132.jpg)
Flow Lines and Folds
Mark visible on the finished item that indicate the direction of flow in the cavity.
![Page 133: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/133.jpg)
Flow Lines and Folds - Problems
• Stock temperature too low.
• Runners too small
• Improper gate size and/or location.
• mould temperature too low.
• Inadequate cold slug well.
![Page 134: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/134.jpg)
Excessive Warpage/ Shrinkage
Excessive dimensional change in a part after processing, or the excessive
decrease in dimension in a part through cooling.
![Page 135: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/135.jpg)
Warpage / Shrinkage -Problems
• mould closed time too short.• Inefficient injection forward
time.• Ram speed too high or too
low.• Injection and holding
pressure too high or low.• Melt temperature
inadequate.• Excessive nozzle and
metering zone temperatures.• mould temperature too high
(for thick wall sections).
• Parts cool unevenly.• Parts underpacked.• Improper gate location.• Gate too restrictive• Unequal temperature
between mould halves.• Non-uniform part ejection.• Parts mishandled after
ejection.• Unbalanced gates on
multiple gated part.• Too many stresses in part.
![Page 136: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/136.jpg)
Black Specks
Particles in the surface of an opaque part and visible throughout a transparent part.
![Page 137: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/137.jpg)
Black Specks - Problems
• Contamination of material. • Holdup of molten resin moulding machine or mould
runner system. • Press Contamination.• Local over-heating in the injection cylinder.• Defective closure of the nozzle.• Oxidation by occluded air or inadequate air venting• mould contains grease.• Trapped air• Inefficient injection speed.
![Page 138: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/138.jpg)
Brittleness
Tendency of a moulded part to break, crack, shatter, etc. under conditions which
it would not normally do so.
![Page 139: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/139.jpg)
Brittleness - Problems
• mould temperature too high• Inadequate cooling in gate area• Gate section of item too thin (gate brittleness)• Resin too cold.• Non-uniformity of resin temperature.• Undried material.• Contamination.• Poor part design.• Material degraded.• Non-compatible mould release.• Packing the mould.• Melt temperature too cold.• Excessive amounts of regrind.
![Page 140: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/140.jpg)
Brittleness - Problems
• Inadequate mould temperature• Excessive screw rpm• Excessive back pressure• Insufficient venting.• Improper gate location.• Excessive injection speed.• Excessive residence timed• Melt temperature too high.• Nozzle too hot.• Injection pressure too low (weld lines).• Runners and gates in adequate (weld lines).• Dwell time in the injection cylinder too long (material degraded).• Material degraded during drying or pre-heating
![Page 141: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/141.jpg)
Flash
Excess plastic around the area of the mould parting line on a moulded
part.
![Page 142: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/142.jpg)
Flash - Problems
• mould parting surfaces do not seal properly.• Injection pressure too high.• Clamp pressure set too low or projected area
or item too large for clamp pressure of the machine.
• Injection temperature too high.• Feed needs adjustment.• Hold time too long.• Inadequate mould supports.• Oversize vents.
![Page 143: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/143.jpg)
Blister
Defect on the surface of a moulded part caused by gases trapped within the part
during curing.
![Page 144: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/144.jpg)
Blister - Problems
• Screw rpm too high
• Back pressure too low
• mould temperature too low.
• Gate improperly located
• Insufficient venting.
• Regrind too coarse
![Page 145: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/145.jpg)
Crazing
Fine cracks in part surface. May extend in a network over the surface
or through the part.
![Page 146: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/146.jpg)
Crazing - Problems
• Insufficient drying of the material.• Contamination.• Injection temperature too high (crazing
accompanied by dis-coloring or yellowing).• mould surface contaminated• Inadequate injection speed.• Inefficient injection forward time.• Excessive injection pressure.• mould temperature too low.• Gate too large.
![Page 147: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/147.jpg)
Cracking
Fracture of the plastic material in an area around a boss, projection, or
moulded insert.
![Page 148: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/148.jpg)
Cracking - Problems
• Parts cool too quickly
• moulded-in stress
• Wall thickness too heavy for compound.
![Page 149: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/149.jpg)
Low Gloss
Surface roughness resulting from high speed fill which causes surface wrinkling
as the polymer melt flows along the wall of the mould.
![Page 150: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/150.jpg)
Low Gloss - Problems
• Inadequate polish of mould surface.
• Material or mould too cold.
• Air entrapment.
• Melt index of material too low.
• Improper mould design.
• Wrong injection pressure.
• Excessive injection speed.
![Page 151: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/151.jpg)
Low Gloss - Problems
• Inadequate flow.
• Contamination
• Resin excessively moist
• Sprue, runners, and/or gate size too small.
• Pigment agglomerates.
• Oil or grease on knockout pins.
![Page 152: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/152.jpg)
Short Shot
Injection of insufficient material to fill the mould.
![Page 153: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/153.jpg)
Short Shot - Problems
• Insufficient feed, cushion.• Inadequate injection pressure.• Inadequate injection speed.• Insufficient booster or injection high-
pressure time.• Inefficient screw delay.• Inadequate injection back pressure.• Melt temperature too low.• Cylinder temperature inadequate.• mould temperature too low.
![Page 154: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/154.jpg)
Short Shot - Problems
• Gates, sprues, and/or runners too small.• Excessive screw flights in metering zone.• Insufficient venting.• Improper gate location.• Melt index of resin too low.• Excessive clearance between non-return
valve and barrel.• Screw bridging.• Injection press of insufficient capacity.
![Page 155: 2. Injection Moulding.ppt](https://reader035.fdocuments.net/reader035/viewer/2022081513/5695d04e1a28ab9b0291e7c4/html5/thumbnails/155.jpg)