Download - Weld defects interpretation

Transcript
  • 7/30/2019 Weld defects interpretation

    1/61

    Copyright 2004 TWI Ltd

    Weld Defects & Repairs

    Radiographic Interpretation

  • 7/30/2019 Weld defects interpretation

    2/61

    Copyright 2004 TWI Ltd

    Faults in Fusion Welds

  • 7/30/2019 Weld defects interpretation

    3/61

    Copyright 2004 TWI Ltd

    Defects which may be detected by visual inspection

    can be grouped under the following headings

    Cracks

    Solid inclusions

    Surface and profiles

    Misalignment (set-up

    irregularities)

    Gas pores and porosity

    Lack of fusion

    Mechanical damage

    Parent material damage

    Miscellaneous

    Faults in Fusion Welds

  • 7/30/2019 Weld defects interpretation

    4/61

    Copyright 2004 TWI Ltd

    Cracks

  • 7/30/2019 Weld defects interpretation

    5/61

    Copyright 2004 TWI Ltd

    Classified by Shape

    Longitudinal

    Transverse

    Branched

    Chevron

    Classified by Position

    HAZ

    Centreline

    Crater

    Fusion zone

    Parent metal

    Cracks that may occur in welded materials are caused

    generally by many factors and may be classified byshape and position, cracks are classed as planar.

    Cracks

  • 7/30/2019 Weld defects interpretation

    6/61

    Copyright 2004 TWI Ltd

    Hydrogen induced cold cracking(HICC)

    Solidification cracking (Hot Tearing)

    Lamellar tearing

    Re heat cracking

    Process Cracks

  • 7/30/2019 Weld defects interpretation

    7/61Copyright 2004 TWI Ltd

    Longitudinal parent metal crack

    Longitudinal weld metal crack Lamellar tearing

    Transverse weld metal crack

    Cracks

  • 7/30/2019 Weld defects interpretation

    8/61Copyright 2004 TWI LtdTransverse crack Longitudinal crack

  • 7/30/2019 Weld defects interpretation

    9/61Copyright 2004 TWI Ltd

    Inclusions

  • 7/30/2019 Weld defects interpretation

    10/61Copyright 2004 TWI LtdRoot piping

    Cluster porosityGas pore

    Blow hole

    Herringbone porosity

    Loss of gas shield

    Damp electrodes

    Contamination

    Arc length too large

    Damaged electrode flux

    Moisture on parent material

    Welding current too low

    Gas pore 1.6mm

    Gas Cavities

  • 7/30/2019 Weld defects interpretation

    11/61Copyright 2004 TWI Ltd

    Root piping

    Porosity

    Gas Cavities

  • 7/30/2019 Weld defects interpretation

    12/61Copyright 2004 TWI LtdCluster porosity Herringbone porosity

  • 7/30/2019 Weld defects interpretation

    13/61Copyright 2004 TWI Ltd

    Slag originates from weldingflux

    MAG and TIG welding

    process produce silicainclusions

    Slag is caused byinadequate cleaning

    Other inclusions includetungsten and copperinclusions from the TIG and

    MAG welding process

    Slag inclusions are defined as a non-metallic inclusion

    caused by some welding process

    Slag inclusions

    Parallel slag linesLack of interun

    fusion + slag

    Lack of sidewallfusion with

    associated slag

    Solid Inclusions

  • 7/30/2019 Weld defects interpretation

    14/61Copyright 2004 TWI Ltd

    Elongated slag linesInterpass slag inclusions

  • 7/30/2019 Weld defects interpretation

    15/61Copyright 2004 TWI Ltd

    Lack of Fusion

  • 7/30/2019 Weld defects interpretation

    16/61Copyright 2004 TWI Ltd

    Incomplete filled groove+ Lack of sidewall fusion

    1

    2

    1. Lack of sidewall fusion2. Lack of inter-run fusion

    Poor welder skill

    Incorrect electrode

    manipulation

    Arc blow

    Incorrect welding

    current/voltage

    Incorrect travel speed

    Incorrect inter-run cleaning

    Lack of Fusion

  • 7/30/2019 Weld defects interpretation

    17/61Copyright 2004 TWI Ltd

    An imperfection at the toe or root of a weld caused by

    metal flowing on to the surface of the parent metalwithout fusing to it

    Contamination

    Slow travel speed

    Incorrect welding technique

    Current too low

    Overlap

  • 7/30/2019 Weld defects interpretation

    18/61Copyright 2004 TWI Ltd

    Toe OverlapFillet weld

    Toe OverlapButt weld

    Overlap

  • 7/30/2019 Weld defects interpretation

    19/61Copyright 2004 TWI Ltd

    Incomplete root fusion

    Incomplete root penetration

    Low Amps/volts

    Large Root face

    Small Root Gap

    Fast Travel Speed

    Incorrect Electrode Angle

    Contamination

    Arc blow

    Weld Root Defects

  • 7/30/2019 Weld defects interpretation

    20/61

    Copyright 2004 TWI Ltd

    Lack of root fusion Lack of root Penetration

    Weld Root Defects

  • 7/30/2019 Weld defects interpretation

    21/61

    Copyright 2004 TWI LtdLack of root penetration Lack of root fusion

  • 7/30/2019 Weld defects interpretation

    22/61

    Copyright 2004 TWI Ltd

    Surface & Profile

  • 7/30/2019 Weld defects interpretation

    23/61

    Copyright 2004 TWI Ltd

    Incomplete filled groove Poor cap profile

    Excessive cap height

    Poor cap profiles and excessive

    cap reinforcements may lead to

    stress concentration points atthe weld toes and will also

    contribute to overall poor toe

    blend

    Weld Profile Defects

  • 7/30/2019 Weld defects interpretation

    24/61

    Copyright 2004 TWI Ltd Incomplete filled grooveExcess cap reinforcement

  • 7/30/2019 Weld defects interpretation

    25/61

    Copyright 2004 TWI Ltd

    Poor stop/starts

    Weld Profile Defects

  • 7/30/2019 Weld defects interpretation

    26/61

    Copyright 2004 TWI Ltd

    Miscellaneous Defects

  • 7/30/2019 Weld defects interpretation

    27/61

    Copyright 2004 TWI Ltd

    Spatter Excessive current

    Damp electrodes

    Contamination

    Incorrect wire feed speed

    when welding with the MAG

    welding process

    Arc blow

    Miscellaneous Defects

  • 7/30/2019 Weld defects interpretation

    28/61

    Copyright 2004 TWI Ltd

    Accidental striking of the arc

    onto the parent material

    Faulty electrode holder

    Poor cable insulation

    Poor return lead clamping

    Arc strike

    Miscellaneous Defects

  • 7/30/2019 Weld defects interpretation

    29/61

    Copyright 2004 TWI Ltd

    An irregular groove at the toe of a weld run in the

    parent metal Excessive amps/volts

    Excessive travel speed

    Incorrect electrode angle

    Excessive weaving

    Incorrect welding technique

    Electrode too large

    Cap & Root Undercut

  • 7/30/2019 Weld defects interpretation

    30/61

    Copyright 2004 TWI Ltd

    Intermittent Cap Undercut

    Cap Undercut

  • 7/30/2019 Weld defects interpretation

    31/61

    Copyright 2004 TWI LtdCopyright 2003 TWI Ltd Cap undercutRoot undercut

    ld f

  • 7/30/2019 Weld defects interpretation

    32/61

    Copyright 2004 TWI Ltd

    Shrinkage groove

    Insufficient weld metal

    deposited in the root pass

    Too fast a cooling rate during

    the application of the root

    bead pass

    Poor welding technique

    A shallow groove caused by contraction in the weldmetal along each side of the penetration bead

    Weld Root Defect

    ld f

  • 7/30/2019 Weld defects interpretation

    33/61

    Copyright 2004 TWI Ltd

    Concave root

    Root faces too large

    Root gap too large

    Excessive back purge pressure

    during TIG welding

    Excessive root bead grinding

    before the application of thesecond pass

    A shallow groove, which may occur in the root of a butt weld

    Weld Root Defect

    W ld R D f

  • 7/30/2019 Weld defects interpretation

    34/61

    Copyright 2004 TWI Ltd

    Concave Root

    Weld Root Defect

    W ld R D f

  • 7/30/2019 Weld defects interpretation

    35/61

    Copyright 2004 TWI Ltd

    Excessive root penetration

    Root faces too small

    Root gap too large

    Excessive amps/volts

    Slow travel speed

    Root penetration bead in excess in accordance with therelevant specification being used

    Weld Root Defect

    W ld R D f

  • 7/30/2019 Weld defects interpretation

    36/61

    Copyright 2004 TWI Ltd

    Weld Root Defect

    Excessive rootpenetration

  • 7/30/2019 Weld defects interpretation

    37/61

    Copyright 2004 TWI LtdCopyright 2003 TWI LtdConcave root Excess root penetration

    W ld R D f

  • 7/30/2019 Weld defects interpretation

    38/61

    Copyright 2004 TWI Ltd

    High Amps/volts

    Small Root face

    Large Root Gap

    Slow Travel SpeedBurn through

    A localized collapse of the weld pool due to excessive

    penetration resulting in a hole in the root run

    Weld Root Defect

    W ld R t D f t

  • 7/30/2019 Weld defects interpretation

    39/61

    Copyright 2004 TWI Ltd

    Weld Root Defect

    Burn Through

    O idi d R t (R t C ki )

  • 7/30/2019 Weld defects interpretation

    40/61

    Copyright 2004 TWI Ltd

    Loss or insufficient backpurging gas

    Most commonly occurs

    when welding stainlesssteels

    Purging gases include

    argon, helium and

    occasionally nitrogen

    Oxidized Root (Root Coking)

    C t Pi

  • 7/30/2019 Weld defects interpretation

    41/61

    Copyright 2004 TWI Ltd

    Crater pipe

    Weld crater

    Crater Pipe

    C t Pi

  • 7/30/2019 Weld defects interpretation

    42/61

    Copyright 2004 TWI Ltd

    Crater pipe is a shrinkage defect and not a gas defect, it

    has the appearance of a gas pore in the weld crater

    Too fast a cooling rate

    Deoxidization

    reactions and liquid to

    solid volume change

    Contamination

    Crater cracks(Star cracks)

    Crater pipe

    Crater Pipe

  • 7/30/2019 Weld defects interpretation

    43/61

    Copyright 2004 TWI Ltd

    Mechanical Damage

    M h i l D

  • 7/30/2019 Weld defects interpretation

    44/61

    Copyright 2004 TWI Ltd

    Mechanical damage can be defined as any surface material

    damage cause during the manufacturing process.This can included damage caused by:

    Grinding

    Hammering

    Chiselling

    Chipping

    Breaking off welded attachments (torn surfaces)

    Using needle guns to compress weld capping runs

    Mechanical Damage

    Mechanical Damage

  • 7/30/2019 Weld defects interpretation

    45/61

    Copyright 2004 TWI Ltd

    Mechanical Damage

    Mechanical Damage/Grinding Mark

    Chipping Marks

  • 7/30/2019 Weld defects interpretation

    46/61

    Copyright 2004 TWI Ltd

    Set-up Irregularities

    Unequal Leg Lengths

  • 7/30/2019 Weld defects interpretation

    47/61

    Copyright 2004 TWI Ltd

    A variation of leg lengths on a fillet weld

    Note: Unequal leg lengths on a fillet weld may be specifiedas part of the design, in which case it will not beconsidered as a defect.

    Unequal Leg Lengths

    Set up Irregularities

  • 7/30/2019 Weld defects interpretation

    48/61

    Copyright 2004 TWI Ltd

    Plate/pipe Linear Misalignment

    (Hi-Lo)

    Angular Misalignment

    Linear misalignment is

    measured from the lowest

    plate to the highest point.

    Angular misalignment is

    measured in degrees

    Set-up Irregularities

    Set up Irregularities

  • 7/30/2019 Weld defects interpretation

    49/61

    Copyright 2004 TWI Ltd

    Linear Misalignment

    Set-up Irregularities

    Set up Irregularities

  • 7/30/2019 Weld defects interpretation

    50/61

    Copyright 2004 TWI Ltd

    Linear Misalignment

    Set-up Irregularities

  • 7/30/2019 Weld defects interpretation

    51/61

    Copyright 2004 TWI Ltd

    Any Questions

    Questions

  • 7/30/2019 Weld defects interpretation

    52/61

    Copyright 2004 TWI Ltd

    QU 1. Give two main causes for the occurrence of a burn through

    QU 2. Give two main causes for the occurrence of excessive rootpenetration on a single-V butt weld

    QU 3. Give five defects, which may occur when welding carbon

    steel using the MMA welding process with the currentsetting to low

    QU 4. Give three possible causes for the occurrence of lack of

    side wall fusion

    QU 5. Sketch the following defects

    a. Lack of root wall fusion b. Lack of root penetration

    c. Incomplete filled groove d. Concave root

    Questions

    Weld Defects

  • 7/30/2019 Weld defects interpretation

    53/61

    Copyright 2004 TWI Ltd

    Material Inspection

    Course notes section references 6

    Material Inspection

  • 7/30/2019 Weld defects interpretation

    54/61

    Copyright 2004 TWI Ltd

    All materials arriving on site should be inspected for:

    Size / dimensions

    Condition

    Type / specification

    In addition other elements may need to be considereddepending on the materials form or shape

    Material Inspection

    Material Inspection

  • 7/30/2019 Weld defects interpretation

    55/61

    Copyright 2004 TWI Ltd

    Parent material defects include:

    Lamination

    Mechanical damage Lap

    Segregation line

    Laminationsare caused in the parent plate by the steel making

    process, originating from ingot casting defects.

    Segregation bandsoccur in the centre of the plate and are low

    melting point impurities such as sulphur and phosphorous.

    Laps are caused during rolling when overlapping metal does not

    fuse to the base material.

    Material Inspection

    Material Inspection

  • 7/30/2019 Weld defects interpretation

    56/61

    Copyright 2004 TWI Ltd

    Material Inspection

    Plate Lamination

    Weld Repairs

  • 7/30/2019 Weld defects interpretation

    57/61

    Copyright 2004 TWI LtdCopyright 2004 TWI Ltd

    Weld Repairs

    Course notes section references 16

    Weld Repairs

  • 7/30/2019 Weld defects interpretation

    58/61

    Copyright 2004 TWI Ltd

    Authorization for repair

    Removal and preparation for repair

    Testing of repair - visual and NDT

    In the event of repair

    Weld Repairs

    Weld Repairs

  • 7/30/2019 Weld defects interpretation

    59/61

    Copyright 2004 TWI Ltd

    A weld repair may be used to improve weld profiles or

    extensive metal removal

    Repairs to fabrication defects are generally easier than

    repairs to service failures because the repair procedure

    may be followed The main problem with repairing a weld is the

    maintenance of mechanical properties

    During the inspection of the removed area prior to welding

    the inspector must ensure that the defects have been

    totally removed and the original joint profile has been

    maintained as close as possible

    Weld Repairs

    Weld Repairs

  • 7/30/2019 Weld defects interpretation

    60/61

    Copyright 2004 TWI Ltd

    The specification or procedure will govern how the defectiveareas are to be removed. The method of removal may be

    Grinding

    Chipping

    Machining

    Filing

    Oxy-Gas gouging

    Arc air gouging

    Weld Repairs

  • 7/30/2019 Weld defects interpretation

    61/61

    Any Questions