Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning...
Transcript of Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning...
![Page 1: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/1.jpg)
Refinery maintenance systems guideTrusted coating solutions
![Page 2: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/2.jpg)
Click on refinery area
Technical helpdesk
![Page 3: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/3.jpg)
Carbon steel, uninsulated 250ºF (121ºC) - 800ºF (426ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 6/Sa 2 Commercial Blast (spot repairs) SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Flare stack
Home Technical helpdesk
![Page 4: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/4.jpg)
DesalterCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 5: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/5.jpg)
Tank lining & secondary containment
HomeHome Technical helpdesk
Lining selection for internal tanks and secondary containment is dependent of various factors such as chemical exposure, temperature, pressure, etc. Please contact your Hempel Technical Department for recommendations by clicking on Technical helpdesk.
![Page 6: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/6.jpg)
Distillation column & splitterCarbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 7: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/7.jpg)
BoilerCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 8: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/8.jpg)
Pumps & compressorsCarbon steel, uninsulated Overcoating OEM suppliers standard paint system. Ambient - 250ºF (121ºC) Surface preparation: Clean in accordance to SSPC-SP 1 Solvent Clean. Sand with 80 Grit Sandpaper. (*Note: Test patch may be required on OEM suppliers standard paint system)
Carbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Home Technical helpdesk
![Page 9: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/9.jpg)
Process vesselCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 10: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/10.jpg)
Heat exchangerCarbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Home Technical helpdesk
![Page 11: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/11.jpg)
Storage tank exteriorCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Home Technical helpdesk
![Page 12: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/12.jpg)
Pipes & valvesCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 13: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/13.jpg)
CokerCarbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 14: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/14.jpg)
HydrocrackerCarbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 15: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/15.jpg)
Carbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
ReformerCarbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast (minimum) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 16: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/16.jpg)
Pipe racks & structural steelCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Aged galvanized steel Ambient - 250ºF (121ºC) Surface preparation: Power wash entire surface in accordance to SSPC-SP 12 WJ-4. SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs)
Home Technical helpdesk
![Page 17: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/17.jpg)
External floating roofCarbon steel, uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 10/Sa 2.5 Near White Metal Blast SSPC-SP 11 Power Tool Cleaning to Bare Metal (minimum)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC) Surface preparation: SSPC-SP 6/Sa 2 Commercial Blast SSPC-SP 2/St 2 or St 3 Hand Tool Cleaning (spot repairs) SSPC-SP 3/St 2 or St 3 Power Tool Cleaning (spot repairs) SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless)
Home Technical helpdesk
![Page 18: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/18.jpg)
Carbon steel, uninsulated Ambient - 250ºF (121ºC)
Product DFT
Hempadur Avantguard 750 2-4 mils / 50-100 microns
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempathane HS 55610 2-3 mils / 50-75 microns
Total DFT 8-15 mils / 200-375 microns
Home Technical helpdesk
![Page 19: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/19.jpg)
Carbon or stainless steel, insulated or uninsulated Ambient - 250ºF (121ºC)
Product DFT
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempathane HS 55610 2-3 mils / 50-75 microns
Total DFT 10-19 mils / 250-475 microns
Home Technical helpdesk
![Page 20: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/20.jpg)
Carbon steel, uninsulated 250ºF (121ºC) - 800ºF (426ºC)
Product DFT
Hempel’s Galvosil 15680 2-3 mils / 50-75 microns
Hempel’s Silicone Aluminum 56913 1-2 mils / 25-50 microns
Total DFT 3–5 mils / 75-125 microns
Home Technical helpdesk
![Page 21: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/21.jpg)
Carbon or stainless steel, insulated or uninsulated Ambient - 400ºF (204ºC)
Product DFT
Hempadur 85671 4-8 mils / 100-200 microns
Hempadur 85671 4-8 mils / 100-200 microns
Total DFT 8-16 mils / 200-400 microns
Home Technical helpdesk
![Page 22: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/22.jpg)
Carbon or stainless steel, insulated -321ºF (-196ºC) - 1,200ºF (649ºC)
Product DFT
Versiline CUI 56990 5-6 mils / 125-150 microns
Versiline CUI 56990 5-6 mils / 125-150 microns
Total DFT 10-12 mils / 250-300 microns
Home Technical helpdesk
![Page 23: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/23.jpg)
Carbon steel, uninsulated Ambient - 250ºF (121ºC)
Product DFT
Vendor supplied coating* n/a
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempathane HS 55610 2-3 mils / 50-75 microns
Total DFT 6-11 mils / 150-275 microns
Home Technical helpdesk
![Page 24: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/24.jpg)
Carbon steel, uninsulated Ambient - 250ºF (121ºC)
Product DFT
Hempadur Avantguard 750 2-4 mils / 50-100 microns
Hempadur Fast Dry 17410 3-5 mils / 75-125 microns
Hempathane HS 55610 2-3 mils / 50-75 microns
Total DFT 7-12 mils / 175-300 microns
Home Technical helpdesk
![Page 25: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/25.jpg)
Aged galvanized steel Ambient - 250ºF (121ºC)
Product DFT
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempadur Mastic 45880 4-8 mils / 100-200 microns
Hempathane HS 55610 2-3 mils / 50-75 microns
Total DFT 10-19 mils / 250-475 microns
Home Technical helpdesk
![Page 26: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/26.jpg)
Stainless steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC)
Product DFT
Versiline CUI 56990 5-6 mils / 125-150 microns
Versiline CUI 56990 5-6 mils / 125-150 microns
Total DFT 10-12 mils / 250-300 microns
Home Technical helpdesk
![Page 27: Refinery maintenance systems guide - Hempel/media/Sites/... · SSPC-SP 16 Brush-off Blast Cleaning of Non-ferrous Metals (stainless) Carbon or stainless steel, insulated or uninsulated](https://reader030.fdocuments.net/reader030/viewer/2022040303/5e87e866639c0132001a497e/html5/thumbnails/27.jpg)
Carbon steel, uninsulated -321ºF (-196ºC) - 1,200ºF (649ºC)
Product DFT
Versiline CUI 56990 7-8 mils /175-200 microns
Versiline CUI 56990 7-8 mils /175-200 microns
Total DFT 14-16 mils / 350-400 microns