NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT,...
Transcript of NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT,...
![Page 1: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/1.jpg)
Warren C. Oliver 1 & George M. Pharr 2
2 University of Tennessee, Dept. of Materials Science and Engineering; &
Oak Ridge National Laboratory, Materials Science & Technology Division
Knoxville, TN
• Research sponsored in part by the Division of Materials Sciences and Engineering, Office of Basic Energy Sciences,
U.S. Department of Energy, and by the National Science Foundation, and the Alexander von Humboldt Foundation.
NANOINDENTATION IN MATERIALS RESEARCH:
PAST, PRESENT, AND FUTURE
1 Nanomechanics Inc., Oak Ridge, TN
Nanomechanics
Inc
![Page 2: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/2.jpg)
OUTLINE
A Brief History
• the instrument (WCO)
• the method for H&E measurement (GMP)
• the obvious applications (GMP)
Some Applications That Weren’t So Obvious
• geology & planetary materials (WCO)
• polymers & viscoelastic materials (WCO)
• the continuum to atomistic bridge (GMP)
• biology & medical science (WCO)
• some unusual applications (GMP)
![Page 3: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/3.jpg)
THE ORIGINAL
NANOINDENTER
![Page 4: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/4.jpg)
THE ORIGINAL NANOINDENTER
• Pethica, Hutchings, and Oliver, Phil Mag A48, 593(1983)
![Page 5: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/5.jpg)
BASIC MEASUREMENTS
65.3°
Berkovich indenter
1 mm
![Page 6: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/6.jpg)
• Pethica, Hutchings and Oliver,
Nuclear Instruments and Methods,
209/210 (1983)
THE ORIGINAL APPLICATION
• Hardness of ion-implanted metals
![Page 7: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/7.jpg)
THE METHOD:
A BRIEF OVERVIEW
![Page 8: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/8.jpg)
KEY PRIOR WORK
N.A. Stillwell & D. Tabor
“Elastic recovery of conical indentations”Proc. Phys. Soc. London 78, 169 (1961)
I.N. Sneddon
“The relation between load and penetration in the axisymmetric
Boussinesq problem for a punch of arbitrary profile” Int. J. Engng. Sci. 3, 47 (1965)
S.I. Bulychev et al.
“Determination of Young’s modulus according to indentation
diagram”Zavod. Lab. 41, 1137 (1975)
J.L. Loubet et al.
“Vickers indentation curves of magnesium oxide (MgO)” J. Tribology 106, 43 (1984)
M.F. Doerner & W.D. Nix
“A method for interpreting the data from depth-sensing indentation
instruments”JMR 1, 601 (1986)
![Page 9: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/9.jpg)
THE FUNDAMENTAL EQUATION
Sneddon, Int J Engrg Sci 3, 47 (1965)
P
hc
ha A
z
r
z = f(x) ; x=r/a
• Pharr, Brotzen, & Oliver, J Mater Res 7, 613 (1992)
P(a)2Eeffax2f'(x)dx
1 x20
1
; Eeff E
1 2
h(a)f'(x)dx
1 x20
1
hc lim2
x2
1yf(y)dy
(y2 x2) 1 y20
1
x 1
S dP
dh 2Eeffa
2
Eeff A
![Page 10: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/10.jpg)
HARDNESS & MODULUS MEASUREMENT
Eeff E
1 2
S
2a
2
S
A
H P
A
A A(hc )
hc hmax Pmax
S(area function)
• Oliver & Pharr, J Mater Res 7, 1564 (1992)
P
h
S=dP/dh
hmax
Pmax
loading
unloading
9.4 mm
65.3°
Berkovich indenter
![Page 11: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/11.jpg)
MONOLITHIC MATERIALS
![Page 12: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/12.jpg)
ASSESSMENT OF METHOD
0
50
100
150
200
250
300
350
400
0 50 100 150 200 250 300 350 400
Nominal valueCuMgMoStainless steelSnTiamorphous SiO2brass
Nan
oin
den
tation
Mo
du
lus,
E (
GP
a)
Conventional Modulus, E (GPa)
![Page 13: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/13.jpg)
OBVIOUS APPLICATIONS
• Surface modified materials
- ion implanted
- laser treated
- radiation damaged
• Thin films
-semiconductor
- magnetic storage
- optical coatings
• Materials of limited size
- powders
- small crystals
• Composite & multiphase materials
• Hard coatings
- machine tool
- thermal spray
- diamond-like carbon (DLC)
• Weldments & joints
9.4 mm
![Page 14: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/14.jpg)
GEOLOGY & PLANETARY
MATERIALS
![Page 15: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/15.jpg)
• Chakoumakos, Oliver, Lumpkin and Ewing, Radiation Effects and
Defects in Solids, 118 (1991)
LONG TERM RADIATION DAMAGE
![Page 16: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/16.jpg)
-10
-9
-8
-7
-6
-5
-4
-3
0
2
4
6
8
10
12
14
16
0 50 100 150 200 250
Hard
nes
s (G
Pa)
Position (microns)
Log D
ose
(10
15
Alp
has/
mg)
Chakoumakos, Oliver, Lumpkin and Ewing, Radiation Effects and
Defects in Solids, 118 (1991)
RADIATION DAMAGED ZIRCON
![Page 17: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/17.jpg)
POLYMERS &
VISCOELASTIC MATERIALS
![Page 18: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/18.jpg)
CONTIUOUS STIFFNESS MEASUREMENT
Elastic
-2
-1
0
1
2
-1
-0.5
0
0.5
1
0 10 20 30 40 50
Exc
itatio
n fo
rce
(µN
)
Response displacem
ent (nm)
Time (milliseconds)
Viscoelastic
-2
-1
0
1
2
-1
-0.5
0
0.5
1
0 10 20 30 40 50
Exc
itatio
n fo
rce
(µN
)
Response displacem
ent (nm)
Time (milliseconds)
= 0°
= 90°
• Oliver & Pethica, US Patent No. 4,848,141, July 1989
![Page 19: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/19.jpg)
Courtesy of Tom Fleischman and Remi Granier, Goodyear Tire & Rubber Co.
45 µm dia. flat punch; 10 Hz
AUTOMOTIVE TIRES
![Page 20: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/20.jpg)
NANOIMPRINT FORMING
Nanometer gap polymer
squeeze flow, 115 °C
• Courtesy of Graham Cross, CRANN, Trinity College Dublin
![Page 21: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/21.jpg)
THE CONTINUUM TO
ATOMISTIC BRIDGE
![Page 22: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/22.jpg)
GETTING “BETWEEN” THE DISLOCATIONS
P
highly stressed zone
L 1
m-2 101210131014
L mm1.00.30.1 • Shim et al, Scripta Mater 59, 1095 (2008)
![Page 23: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/23.jpg)
POP-IN & THE THEORETICAL STRENGTH
• Page, Oliver, and McHargue J Mater Res 7, 450 (1992)
Hertzian AnalysisP
•
aR
0.48a45°
h
At pop-in:
max theo G / 30G / 5
e.g.: Al2O3, W, Ni3Al, Au,
Cu, Al, Ni, Mo5SiB2,
CaF2, etc.
max 0.31pm 0.316PEr
2
3R 2
1/ 3
80 nm 350 nm
Berkovich
(001) sapphire
pop-in
Displacement, h (nm)
Load, P
(m
N)
65.3°
0 100 200 300
30
20
10
0
Displacement, h (nm)
loading
unloading
Load, P
(m
N)
0 20 40 60 80
8
6
4
2
0
![Page 24: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/24.jpg)
ATOMISTIC MODELING
• courtesy Prof. A. Hartmaier,
Ruhr University Bochum
P
(111) copper single crystal
2.5x106 atoms; (30 nm)3
R = 8 nm; h = 2 nm
Molecular Dynamics Simulation
![Page 25: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/25.jpg)
THE INDENTATION SIZE EFFECT
P1
A1
P2 > P1
A2
Hardness:
H P
A
Smaller is stronger !
Ma & Clarke, J Mater Res. 10, 853 (1995)
Single Crystal Silver
conventional plasticity
Berkovich
65.3°
![Page 26: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/26.jpg)
BIOLOGY &
MEDICAL SCIENCE
![Page 27: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/27.jpg)
CORTICAL vs. TRABECULAR BONE
Interstitial lamellae
Cortical(dense, compact)
osteon
Transverse section
trabecular struts
Trabecular(spongy, cancellous)
• Turner et al, J Biomech 32, 437 (1999)
transverse section
trabecular
bone
cortical bone
osteon
10-500 mm
Specimen E (GPa)
Acoustic
E (GPa)
Nanoindentation
trabecular 17.2 18.2 ± 0.5
cortical (transverse) 15.1 16.6 ± 0.3
cortical (longitudinal) 20.9 23.4 ± 0.6
![Page 28: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/28.jpg)
WOOD CELL WALLS
cellulosic
microfibrils
• Konnerth et al, J Mater Sci 44, 4399 (2009)
![Page 29: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/29.jpg)
SOME UNUSUAL
APPLICATIONS
![Page 30: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/30.jpg)
HYDROTHERMAL VENT GASTROPODS
• Yao et al, PNAS 107, 987 (2010)
“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”
![Page 31: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/31.jpg)
HYDROTHERMAL VENT GASTROPODS
• Yao et al, PNAS 107, 987 (2010)
“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”
C. Squamiferum (2001)
![Page 32: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/32.jpg)
HYDROTHERMAL VENT GASTROPODS
• Yao et al, PNAS 107, 987 (2010)
“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”
C. Squamiferum (2001) Vent crab
![Page 33: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/33.jpg)
HYDROTHERMAL VENT GASTROPODS
• Yao et al, PNAS 107, 987 (2010)
“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”
C. Squamiferum (2001) Vent crab
![Page 34: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/34.jpg)
HYDROTHERMAL VENT GASTROPODS
• Yao et al, PNAS 107, 987 (2010)
“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”
Armor Mechanics (FEM)
OL: Fe-based granular
• tough
• abrades penetrator
ML: organic
• compliant
• arrests cracks
• protects brittle ILIl: calcified shell
• structural support
• fatigue/bendiing resistance
C. Squamiferum (2001) Vent crab
![Page 35: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/35.jpg)
THE LAACHER SEE HYPOTHESIS
• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)
“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”
![Page 36: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/36.jpg)
THE LAACHER SEE HYPOTHESIS
• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)
“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”
![Page 37: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/37.jpg)
THE LAACHER SEE HYPOTHESIS
• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)
“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”
~11,000 BC
![Page 38: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/38.jpg)
THE LAACHER SEE HYPOTHESIS
• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)
“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”
~11,000 BC
![Page 39: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/39.jpg)
TESTING THE HYPOTHESIS
red deer tooth
Er
dentinenamel
H
Hard
ne
ss, H
(G
Pa
)
Mo
du
lus. E
r(G
Pa
)
Location (mm)
Hardness (GPa)
Hardness
Particle
Ash
![Page 40: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/40.jpg)
TESTING THE HYPOTHESIS
red deer tooth
Er
dentinenamel
H
Hard
ne
ss, H
(G
Pa
)
Mo
du
lus. E
r(G
Pa
)
Location (mm)
Hardness (GPa)
Hardness
Particle
Ash
![Page 41: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …ksm.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura/Oliver... · 2011. 3. 1. · NANOINDENTER. THE ORIGINAL NANOINDENTER •Pethica,](https://reader035.fdocuments.net/reader035/viewer/2022071408/610067a23813ed464a087df2/html5/thumbnails/41.jpg)
Thanks for your attention !!