Metakaolin presentation

26
Cement/Fly Ash /Metakaolin Ternary Blends: Effects on Compressive Strengths of Mortars and Economics Presented By: Billy Wiggins, P.E., Associate Member ACI Committee 232

description

 

Transcript of Metakaolin presentation

Page 1: Metakaolin presentation

Cement/Fly Ash /Metakaolin Ternary Blends: Effects on Compressive Strengths of Mortars and Economics

Presented By: Billy Wiggins, P.E., Associate Member ACI Committee 232

Page 2: Metakaolin presentation

Points of Discussion

Pozzolans Experiment Design Experiment Results Conclusion

Page 3: Metakaolin presentation

Pozzolans

ACI Definition Pozzolanic Reactions Fly Ash Silica Fume Metakaolin Ternary Blends

Page 4: Metakaolin presentation

ACI Definition

A siliceous or alumino- siliceous material that, in finely divided form and in the presence of moisture, chemically reacts with calcium hydroxide released by the hydration of Portland cement to form compounds possessing cementing properties.

Page 5: Metakaolin presentation

Pozzolanic Reactions

2C3S + 6H C3S2H3 + 3CH

2C2S + 4H C3S2H3 + CH Hydration of Calcium Silicates Calcium Hydroxide (CH) is weak and porous

by itself Pozzolans react with CH to form C-S-H

Page 6: Metakaolin presentation

Improved Aggregate-Cement Interface Pozzolan Acts as

Micro-filler Increases Bond Leads to Higher

Strength

Page 7: Metakaolin presentation

Fly Ash

A By-Product from the Combustion of Pulverized Coal

Small glassy beads 10m Average Particle Diameter Cheap… $30/ton Versus Cement at $85/ton 90% still goes to Land Fill

Page 8: Metakaolin presentation

Fly Ash Properties in Cement Improved Workability Improved Long-Term Strength Gains Price Lowers Heat of Hydration Decreases Water Demand Less Bleeding Improved Durability to ASR, Sulfate, &

Chlorides

Page 9: Metakaolin presentation

Silica Fume

Produced from the Production of Silicon 93% SiO2

.1m Average Particle Diameter

Page 10: Metakaolin presentation

Properties of Silica Fume

Greatly Improves Compressive Strengths Decreased Porosity Increases Water Demand (HRWR Typ.) “Sticky” finish Decreases Workability Decreases Bleeding Improved Durability to ASR, Sulfate, &

Chlorides

Page 11: Metakaolin presentation

Metakaolin

Produced from Kaolin Crude Clays An Engineered Product 1 m in diameter Plate-Like in Shape Kaolin Mined in Middle Georgia SiO2 + Al2O3 + TiO2 +Fe2O3

Page 12: Metakaolin presentation

Properties of Metakaolin Increased Water Demand (125%) Product “Creamy” Greatly Improves Compressive Strengths.

Comparible or Better than SF Improved Durability (ASR and Sulfate) Increases Heat of Hydration Decreases Bleeding Improved Durability to ASR, Sulfate, &

Chlorides

Page 13: Metakaolin presentation

Ternary Blends Flyash+Cement+Metakaolin or Silica Fume Less HRWR Less Sticky Good Early Age and Increased Later-Age

Strength Lower Heat Rise Improved Durability to ASR, Sulfate, &

Chlorides – Better than Single Blends?

Page 14: Metakaolin presentation

Improved Particle Packing

Page 15: Metakaolin presentation

Improved Workability

Page 16: Metakaolin presentation

Experiment Design

Data on SF + FA; Not much on MK+FA Synergy Between MK and FA ? Economics ? Standard ASTM Tests Maintained Flowability

Page 17: Metakaolin presentation

Mix Matrix % Repalcement of Cement

Metakaolin

0 5 10

Flyash

0 0/0 0/5 0/10

1515/0 5/15 10/15

3030/0 5/30 10/30

Page 18: Metakaolin presentation

RecipesRecipes for Cement Mortars

Mix #1 Mix #2 Mix #3 Mix #4 Mix #5 Mix #6 Mix #7 Mix #8 Mix #9

%MK 0 0 0 0.05 0.1 0.05 0.1 0.05 0.1

%FA 0 0.15 0.3 0 0 0.15 0.15 0.3 0.3

Sand (g) 2035 2035 2035 2035 2035 2035 2035 2035 2035

Cement (g) 740 629 518 703 666 592 555 481 444

Water (g) 359 345.6 332.1 363.4 368.0 350.0 354.4 336.5 341.0

Flyash (g) 0 111 222 0 0 111 111 222 222

Metakaolin (g) 0 0 0 37 74 37 74 37 74

W/(C+Pozz) Ratio 0.49 0.47 0.45 0.49 0.50 0.47 0.48 0.45 0.46

Flow % Increase 0.52 0.50 0.54 0.52 0.53 0.48 0.44 0.45 0.41

Page 19: Metakaolin presentation

Compressive Strength vs. Curing Time

0

1000

2000

3000

4000

5000

6000

7000

8000

0 10 20 30 40 50 60

Days

PS

I

Control Mix15%FA30%FA5%MK10%MK5%MK - 15%FA10%MK - 15%FA5%MK - 30%FA10%MK - 30%FA

Page 20: Metakaolin presentation

Cost Analysis INational Average: Ready Mix

Concrete Strength vs. Cost per CY

Information from Means Building Construction Cost Data 60thEd.

$0.00

$10.00

$20.00

$30.00

$40.00

$50.00

$60.00

$70.00

$80.00

$90.00

$100.00

2000 2500 3000 3500 4000 4500 5000 5500 6000 6500

compressive strength

cost

per

yar

d

Page 21: Metakaolin presentation

Cost Analysis II Cost Comparison of Blends @ 28 Day Compressive Break Strengths

Mix #1(CM)

Mix #2 Mix #3 Mix #4 Mix #5 Mix #6 Mix #7 Mix #8 Mix #9

%MK 0 0 0 0.05 0.1 0.05 0.1 0.05 0.1

%FA 0 0.15 0.3 0 0 0.15 0.15 0.3 0.3

Sand 2035 2035 2035 2035 2035 2035 2035 2035 2035

Cement 740 629 518 703 666 592 555 481 444

Fly ash 0 111 222 0 0 111 111 222 222

Metakaolin 0 0 0 37 74 37 74 37 74

cost for 1 ton of mortar 32.19 30.00 27.80 37.73 43.26 35.53 41.06 33.33 38.86

28d Fc 4,652 4467 3433 5759 6128 5131 5648 4135 3839

cost of a ton of mortar/psi 6.92 6.71 8.10 6.55 7.06 6.92 7.27 8.06 10.12

Page 22: Metakaolin presentation

Cost Analysis III

0

1,000

2,000

3,000

4,000

5,000

6,000

7,000

Mix #1(CM) Mix #2 Mix #3 Mix #4 Mix #5 Mix #6 Mix #7 Mix #8 Mix #9

Mixture

28d

Com

pres

sive

Str

engt

h (p

si)

Page 23: Metakaolin presentation

Cost Analysis IV

0.00

5.00

10.00

15.00

20.00

25.00

30.00

35.00

40.00

45.00

50.00

Mix #1(CM) Mix #2 Mix #3 Mix #4 Mix #5 Mix #6 Mix #7 Mix #8 Mix #9

Mixture

Co

st f

or

1 to

n o

f M

ort

ar

Page 24: Metakaolin presentation

Cost Analysis V

0.00

2.00

4.00

6.00

8.00

10.00

12.00

Mix #1(CM) Mix #2 Mix #3 Mix #4 Mix #5 Mix #6 Mix #7 Mix #8 Mix #9

Mixture

Co

st (

$) f

or

1 to

n o

f M

ort

ar/p

si

Page 25: Metakaolin presentation

Conclusion Fly Ash Lowers Water Demand in Ternary

Blends. Metakaolin Has Better Compressive Strength

Properties Alone than in Ternary Blends in Mortar (24% Stronger at 28d than CM).

Metakaolin has Improved “Finishability” over control mixes.

The use of 5% Metakaolin lessens the cost of a mortar mixture 5.35% per psi.

Page 26: Metakaolin presentation

Questions?