Du Pont Titanium Dioxide - Assumptions. Du Pont Titanium Dioxide - Do Nothing.
Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer...
Transcript of Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer...
![Page 1: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/1.jpg)
Atomic Layer Deposition Coating Titanium Dioxide
Nano-thin Film on Magnesium-Zinc Alloy to Enhance
Cytocompatibility for Vascular Stents
A Thesis Presented
By
Fan Yang
to
The Department of Chemical Engineering
in partial fulfillment of the requirements
for the degree of
Master of Science
in the field of
Chemical Engineering
Northeastern University Boston, Massachusetts
December 15th, 2018
![Page 2: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/2.jpg)
ACKNOWLEDGEMENTS
First of all, I would like to thank my advisor, Dr. Thomas J. Webster, for his
invaluable guidance, support and encouragement to my research work. I am always
appreciative of this precious opportunity to work in the Webster Nanomedicine
Laboratory and to learn from him about all research aspects, starting from experimental
design, problem solving, divergent thinking, and finally to be a professional scientist.
He led me into the world of nanomedicine and his passion in research inspires me to
work hard, make efforts and go beyond my own continuously. Without his help and
effort, I could not achieve what I have today. The lessons I have learned from him will
benefit my whole life.
I would like to thank Dr. Guohao Dai and Dr. Ryan Koppes for attending my
thesis defense as committee members and offering constructive suggestions to my
research. I would like to thank the George J. Kostas Nanoscale Technology and
Manufacturing Research Center (Northeastern University) and Center for Nanoscale
Systems (Harvard University) for providing the facilities for material characterization.
Also, I truly appreciate William Fowle for his technical assistance with microscopy and
Robert Eagan for sample preparation.
![Page 3: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/3.jpg)
2
Many thanks to current and former members of the Webster Nanomedicine lab
for providing countless support and making me feel so warm being a part of the big
family. In particular, I want to thank Run Chang for leading me through my entire
project and providing constructive advises. Also, I specially want to thank Catherina B.
Garcia, Di Shi, Guijie Mi, Jieda Chen, Junyan Zhang, Luting Liu, Ming Gao, Zelong
Xie, Nicole Bassous, Paria Ghannadian, James Moxley, and Bohan Zhang for their help
in my research. I truly appreciate all of your help and effort! With great gratitude, a
huge thank you goes to my parents for their unconditional support and love.
Finally, I would like to thank Northeastern University for funding.
![Page 4: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/4.jpg)
3
TABLE OF CONTENT
List of Figures ................................................................................................. 4
List of Tables .................................................................................................. 4
Abstract .......................................................................................................... 5
1. Introduction ................................................................................................ 7 1.1 Overview ......................................................................................................... 7 1.2 Statement of the Problem ............................................................................... 12
2. Materials and Methods ............................................................................ 15 2.1 Magnesium-Zinc Platform ............................................................................. 15
2.2 TiO2-Coated Sample Preparation ................................................................... 15 2.3 Surface Characterization ................................................................................ 17
2.4 Protein Adsorption Assays ............................................................................. 18
2.5 Cell Assays .................................................................................................... 19 2.5.1 Cell Culture ............................................................................................ 19
2.5.2 Fluorescent Microscopy Assays .............................................................. 19
2.5.3 Cell Adhesion and Proliferation Assays .................................................. 20
2.6 Statistics ........................................................................................................ 21
3. Results ....................................................................................................... 22 3.1 Surface Characterization ................................................................................ 22
3.2 Protein Absorption Effect .............................................................................. 26 3.3 Fluorescent Microscopy Assays ..................................................................... 27
3.4 Cell Assays .................................................................................................... 30
4. Discussion ................................................................................................. 32
5. Conclusion and Recommendations .......................................................... 39
6. References ................................................................................................. 41
7. Appendix ................................................................................................... 47
![Page 5: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/5.jpg)
4
LIST OF FIGURES
Figure 1. Precursor schematic principle of ALD using TDMATi and H2O to coat
TiO2 nano-thin film ....................................................................................... 15
Figure 2. Simplified schematic of a typical research-grade viscous flow atomic
layer deposition reactor designed for coating flat samples .......................... 16
Figure 3. SEM image of (A) Mg-Zn Control, (B) Mg-Zn-TiO2 (150°C), (C) Mg-
Zn-TiO2 (200°C) ............................................................................................ 23
Figure 4. XPS graphs for titanium scan of Mg-Zn alloy control and Mg-Zn-TiO2
coating at 150˚C and 200˚C ........................................................................... 25
Figure 5. XRD patterns of Mg-Zn alloy control and Mg-Zn-TiO2 coating at
150˚C and 200˚C ............................................................................................ 25
Figure 6. Water contact angle measurements on Mg-Zn alloy samples with
different TiO2 ALD coatings temperatures .................................................. 26
Figure 7. The amount of adsorbed bovine serum albumin (BSA) protein on
sample surfaces after 24 hours of culture in a 0.01% BSA solution ............ 27
Figure 8. Fluorescent microscope image of (A) Mg-Zn Control, (B) Mg-Zn-TiO2
(150°C), (C) Mg-Zn-TiO2 (200°C) ................................................................. 29
Figure 9. Human coronary endothelial cell proliferation on Mg-Zn alloy control
and Mg-Zn-TiO2 (150 °C, 200 °C) samples .................................................. 31
Figure 10. EDAX data results for Mg-Zn alloy control ....................................... 47 Figure 11. EDAX data results for Mg-Zn-TiO2-150 ˚C ....................................... 48
Figure 12. EDAX data results for Mg-Zn-TiO2-200 ˚C ....................................... 48
LIST OF TABLES
Table 1. Elemental concentrations of Mg-Zn alloy samples before and after ALD
by EDAX ........................................................................................................ 23
![Page 6: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/6.jpg)
5
ABSTRACT
Implantable medical devices are designed to replace missing or restore damaged
biological structures. A coronary stent is a well-known cardiovascular medical device
implanted to resolve disorder of the circulatory system due to bloodstream narrowing
that occurs in coronary arteries. Since the implanted device interacts with surrounding
biological environments, surface structure of a typical implantable device plays a
critical role. Cell adhesion and proliferation performances and protein adsorption are
fundamental identifications for the success of a medical device. Metallic coronary
stents are commonly used as biomaterial platforms in cardiovascular implants. As the
new generation of coronary stents such as bioresorbable vascular scaffolds appears to
attract attentions among researchers, studies of bioresorbable materials such as
magnesium and zinc remains a target for further optimizations. Additional surface
modification is needed to control biodegradation of the implant material while
promoting biological reactions without the use of drug elution. Herein, precise
temperature and thickness controlled atomic layer deposition (ALD) were utilized to
provide a unique and conformal nanoscale TiO2 coating on a customized magnesium-
zinc alloy. Impressively, results indicated that this TiO2 nano-thin film coating
![Page 7: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/7.jpg)
6
stimulated coronary arterial endothelial cell adhesion and proliferation with additional
features like acting as a protective barrier. Data revealed that both surface morphology
and surface hydrophilicity together contributed the ALD nanoscale coating, which
acted as a protection layer inhibiting degradation of the magnesium-zinc substrate.
Additionally, different surface properties and their influences on biological functions
were also investigated. Overall, the outcome of this study provided a promising tissue
regeneration platform with unique nano-structural surfaces to be bioresorbable to
enhance biocompatibility, and as a result will be beneficial for numerous biomedical
applications.
![Page 8: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/8.jpg)
7
1. INTRODUCTION
1.1 Overview
Heart arteries can be blocked or narrowed by a buildup of plaque which results in
the reduction of blood flow to the heart and cause chest discomfort. In some cases,
blood clots can suddenly form inside the artery to cause a completely block of the blood
flow which leads to a heart attack. If coronary artery narrowing occurs, a stent may be
required to reopen the blocked artery. Coronary stents are widely used in coronary
artery heart disease treatments keeping arteries open to support blood supply. The
clinical surgery procedure is called Percutaneous Coronary Intervention (PCI) which
requires a guideline to lead coronary stents to the place where plaque forms on the
artery inner wall and coronary artery shrinkage occurs. Then the coronary stents expand
to compress the plaque to restore normal blood flow inside the coronary arteries.
Coronary stents are now used in more than 90% of PCI procedures 1 and have evolved
from balloon angioplasty to bare metal stents (BMS) then drug-eluting stents (DES)
and now to bioresorbable vascular scaffolds (BVS). The revolutionized treatment of
coronary artery disease, balloon angioplasty, was initially without stent deployment 2.
With the clinical outcome of re-narrowing of coronary arteries due to acute vessel
![Page 9: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/9.jpg)
8
closure, bare metal stents were created to contemporarily support narrowed arteries.
The first Food and Drug Administration (FDA) approved balloon-expandable slotted
tube device, Palmaz-Schatz®, was invented by Johnson & Johnson 3. The bare metal
device was made of stainless steel and remained one of the most studied and widely
used stent in 1990s. However, BMS had high metallic density which resulted in a high
risk of sub-acute stent thrombosis. The technically challenges to implant BMS during
1990s also resulted in frequent surgery failures of stent placement and embolization 4.
After upgrades for both surgical and stent device technologies, DES brought a new
revolution to the interventional cardiology. DES were BMS coated with anti-
proliferative drugs such as sirolimus, paclitaxel, or everolimus which can substantially
reduce the rate of in-stent restenosis compared with BMS 5.
Currently, permanent metal and polymer scaffolds are implanted into coronary
arteries to function as a long-term (>1 year) vascular stents. However, chronic or long-
term clinical issues may occur due to the toxicity of implant materials since these
materials cannot be safely absorbed by the human body. For example, contemporary
metallic drug-eluting stents have great clinical outcomes within 1 year of implantation.
![Page 10: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/10.jpg)
9
After 1 year, stent-related adverse events may appear such as thrombosis, restenosis,
and even myocardial infarction in the arteries. Additionally, chronic inflammation,
neoatherosclerosis, and strut fracture may affect the whole human body. Further
surgery may be required to remove the stent putting risk for plaque buildup requiring
more stents to be placed in the artery 5. BVS is an alternative solution specially designed
for stent implantation as the scaffold can be fully absorbed by the human body safely
without the need of secondary surgeries to remove permanent stents putting the risk of
further chronic diseases.
The complete life cycle of BVS includes three phases: revascularization,
restoration, and resorption. Revascularization involves alleviating coronary stenosis
ischemia-production which is similar to DES when drug elution occurs within the first
5-6 months. Restoration is when the scaffold starts to experience mass loss followed by
a reduction molecular weight after 6 months of implantation. Finally, depending on the
degradation rate of the stent, the resorption process can take up to 2-4 years. Recovery
of vascular structure and function occurs within the revascularization process. After the
BVS has finished its functionality to remodel the coronary artery, it starts to disappear
![Page 11: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/11.jpg)
10
throughout the next two phases of the BVS life cycle. The FDA has approved only one
BVS invented by Abbott 6 with poly (lactic acid) (PLLA) as the stent platform. This
BVS has been reported to show positive vessel remodeling and plaque regression
during the resorption process between 1 and 5 years after implantation 7,8. However,
polymeric stents in general have a lower tensile strength, reduced stiffness, and reduced
ductility compared to metallic stents. Also, polymeric DES has been reported to have
late thrombosis clinical issues 5. On the other hand, metallic biomaterials are very
popular for biomedical application researches.
There is enormous interest for magnesium (Mg) alloys among researchers for
industrial and biomedical application because of their great mechanical properties and
biocompatibility. Magnesium ions in these alloys participate in many metabolic
reactions and biological mechanisms. The large number of magnesium ions present in
the human body are considered to be biocompatible. Normally, the human body contain
approximately 35 g of Mg per 70 kg of body weight and the daily intake of Mg is 375mg
9. The key feature of Mg for biomedical applications is that it is biodegradable. This
feature may be very important when considering Mg as the platform for a BVS.
![Page 12: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/12.jpg)
11
Magnesium alloys have advantages over traditional ceramics, biodegradable polymers,
and other metallic materials. With its excellent mechanical properties of lightweight,
high mechanical strength, and high fracture toughness, many types of Mg stents have
been used by many companies since 2004.
Biotronik introduced three generations of the absorbable metal stent (AMS) with
WE43 magnesium alloy as the platform. The first clinical study result reported for the
coronary arteries of 63 patients to have the AMS safely degraded after 4 months. The
third generation of AMS was coated with degradable polymer carrier with
antiproliferative drug and showed positive results of safety and efficacy compared to
previous AMS during in vivo trials 10. However, WE43 still contains 4% Yttrium and
2.25% Rare earth which can be considered to be toxic or hepatotoxic to human bodies.
In order to develop new generations of BVS, new materials should be non-toxic or low
toxic for biomedical materials to be implanted into the human body.
![Page 13: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/13.jpg)
12
1.2 Statement of the Problem
In this article, magnesium-zinc (Mg-Zn) binary alloy coated with a nano-film
coating technology was used to develop a potential new platform for BVS. Zinc (Zn)
as one of the most abundant nutritionally essential elements in the human body exists
in all human tissues 11. Aside from the physiologically essential need of the element,
zinc also exhibited strong antiatherogenic properties 12. Furthermore, zinc is used to
improve mechanical properties of magnesium for commercial applications. It has been
reported that the viscera histology examination and biochemical measurements proved
the degradation products of Mg-Zn would not damage major organs and Mg-Zn alloy
had good biocompatibility during in vitro cytotoxicity tests with L929 cell lines 13,14.
Nevertheless, the downside of Mg-Zn binary alloy is critical with a high corrosion rate
in vitro and in vivo 10. In order to slow down initial corrosion rate of Mg-Zn alloy,
surface modifications with coating technologies are recommended. To allow implants
to biodegrade and absorb by human body completely at the end, the coatings should act
as a corrosion barrier to cease corrosion at different stages 15.
Ideally, the coatings should also degrade gradually in order to control the overall
corrosion rate of the implant device and leave no harm to human body throughout the
![Page 14: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/14.jpg)
13
entire process. Possible coating technologies for biomaterials include metal-metal
coatings, chemical vapor deposition (CVD), ion beam assisted deposition (IBAD),
Atomic Layer Deposition (ALD), pulsed laser deposition (PLD) and etc. Coating
technologies such as IBAD and PLD will require a line of sight for deposition which is
limited for complex shapes 16,17. On the other hand, Atomic Layer Deposition provides
a uniform, chemically-bonded, pinhole-free and controlled thickness coating on
individual primary surfaces. Since ALD is independent of line of sight, internal
structures under surfaces can also be coated conformally. Even though CVD, similar to
ALD, can also deposit a chemically bonded coating with a vapor deposition, ALD has
the unique ability to split binary reactions into two self-limiting half-reactions occur on
the substrate surface 18. Besides, ALD reactions are self-terminating with precise
thickness controlled by deposition cycles and with good reproducibility applicable to
sensitive substrates such as biomaterials 19. In this study, ALD was chosen to deposit
nanoscale thin film coating on structural Mg-Zn binary alloys. As for the precursor used
for ALD coating on the substrates, Tetrakis(dimethylamido)titanium (TDMATi) was
chosen to deposit titanium dioxide (TiO2). Because TiO2 has shown its good corrosion
![Page 15: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/15.jpg)
14
resistance ability on steel surfaces using the sol-gel method, it can become a protective
barrier for the substrates 20. ALD coating TiO2 was previously used for a 316LVM steel
base to be considered for the application of vascular stents with coating temperature
modified in order to compare mechanical properties of different samples. The results
showed an increase in temperature had an adverse effect on corrosion resistance and a
temperature above 300 °C will significantly decrease material hardness 21. Thus, for
this study, coating temperatures were chosen to deposit TiO2 at 150 °C and 200 °C to
conduct with further material testing experiments. The precursor schematic principle is
shown in Figure 1. Both TDMATi and H2O were purged into the reaction chamber in
order to chemically bond TiO2 to the substrate (Mg-Zn). Biocompatibility experiments
and surface morphology characterizations were tested for Mg-Zn alloys coated with
TiO2 by ALD. The control samples were Mg-Zn alloys without ALD treatments.
![Page 16: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/16.jpg)
15
Figure 1. Precursor schematic principle of ALD using TDMATi and H2O to coat
TiO2 nano-thin film19
2. MATERIALS AND METHODS
2.1 Magnesium-Zinc Platform
Magnesium alloy (ZK61M) plates (1 mm thickness) were customized to only
include Mg and Zn without impurity substances. Samples were purchased from Kaiqi
Mold Steel Ltd., Dongguan China. The ALD instrument was sponsored by Ultratech,
Inc. (Waltham, MA).
2.2 TiO2-Coated Sample Preparation
Mg-Zn alloy samples were cut into identical pieces (0.5 inch × 0.5 inch).
Samples were cleaned with 100% isopropyl alcohol (IPA) and 70% ethanol for 20
minutes respectively. Then, samples were dried at 100 °C inside an oven for 10 minutes.
![Page 17: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/17.jpg)
16
The cleaned samples were placed into a preheated ALD chamber. A vacuum pump was
used to create a vacuum inside the reaction chamber. Titanium dioxide (TiO2) thin films
were deposited onto the Mg-Zn substrates using TDMATi and H2O as ALD precursors.
Nitrogen gas was served as a purging gas fed to the chamber during the entire coating
process. In this study, a single standard ALD cycle is consisted of 0.1 s exposure to
TDMATi, 10 s of N2 purge, 0.015 s exposure to H2O, and again 10 s of N2 purge
repeatedly. The total flow rate of the N2 was 100 standard cubic centimeters per minute
(sccm). The TiO2 thin films were deposited at two different temperatures, 150 °C and
200 °C. For 100 nm of the TiO2 coatings to be applied on Mg-Zn alloys, 2500 cycles
were used to complete the recipe since 0.4 Å was coated per cycle. A simple schematic
of the ALD chamber system is shown in Figure 2.
Figure 2. Simplified schematic of a typical research-grade viscous flow atomic
layer deposition reactor designed for coating flat samples. The red arrows
indicate the flow across samples 22.
![Page 18: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/18.jpg)
17
All samples, including control samples (alloy without ALD), were sonicated with 100%
IPA and 70% ethanol before ALD trials. UV irradiation (60 minutes) were used to
sterilize samples for further biological experiments.
2.3 Surface Characterization
The surface morphology of the samples was characterized by scanning electron
microscopy (SEM, Hitachi S-4800). The qualitative and quantitative analysis of
titanium scans for samples soaked in medium for 0 and 3 days was conducted using an
X-ray Photoelectron Spectroscopy (XPS, XRA008 Thermo Scientific K-alpha+XPS
System) with the data analysis software Avantage. Compositional analysis was
conducted using an Energy-dispersive X-ray Spectroscopy (EDAX, Hitachi S-4800).
The crystallinity of the TiO2 layers was investigated using an X-ray Diffractometer
(XRD, Ultima, Rigaku Corp.) fitted with a Cu Kα radiation. The XRD was operated at
40 kV and 44 mA with a step width of 0.1 θ and a count time of 0.5 s. The scanning
range (2θ) of the XRD trial was 20-90 °. Phase identification was performed using the
standard JCPDS database. To assess samples surface wettability, water contact angles
were measured using a ProScope HR Microscope at room temperature. A droplet of
![Page 19: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/19.jpg)
18
deionized water was added to each sample surface. Three identical samples were
measured to calculate contact angle results.
2.4 Protein Adsorption Assays
Bicinchoninic acid (BCA) protein assay kit (Thermo Scientific) was used to
quantify the total amount of Bovine serum albumin (BSA) protein adsorbed onto the
sample surfaces. 1 mg/mL (0.1%) BSA solution was prepared by diluting 30% BSA
with PBS. Each sample was treated with 1 mL 0.1% BSA solution and cultured for 24
hours in an incubator (37 °C, humidified, 5% CO2). After that, BSA solution is aspirated
and each sample was washed with 1 mL PBS to remove non-adsorbed proteins. Then,
each sample was treated with 1 mL RIPA buffer (Sigma-Aldrich) for 10 minutes to
solubilize adsorbed proteins. A working reagent (WR) was prepared using BCA protein
assay kit with a 50 : 1 ratio of Reagent A : B. According to the BCA assay microplate
protocol, the desired amount of BSA final concentration was mixed with the
corresponding WR and put into a dry bath at 37°C. Finally, 200 μL of each sample BSA
was transferred to a 96-well tissue culture plate and tested at 562 nm by the plate reader
(Molecular Devices, SpectraMax M3).
![Page 20: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/20.jpg)
19
2.5 Cell Assays
2.5.1 Cell Culture
Human Coronary Artery Endothelial Cells (HCAECs, PromoCell, C-12221) were
used for all mammalian cell experiments. Endothelial cells were cultured in Endothelial
Cell Growth Medium (PromoCell, C-22010) with an endothelial cell growth medium
supplemental mix (PromoCell, C-39215) added to the growth medium. Additional 5mL
1% penicillin/ streptomycin (P/S; Sigma-Aldrich) was added to the Endothelial Cell
Growth Medium and filtered to be stored in a 4 °C fridge. All cells were incubated in a
37 °C, humidified, 5% CO2 and 95% air environment.
2.5.2 Fluorescent Microscopy Assays
Cell adhesion samples were prepared and seeded with 100,000 cells per well. After
4 hours of incubation, the samples were washed three times with PBS and then stained
for fluorescence microscopy analysis. A 3.7% formaldehyde solution was used to fix
cells on samples. The samples were further permeabilized with 0.1% Triton X-100
solution for 5 minutes. Rhodamine and Hoechst (Life Technologies) actin stain dyes
were used to view adherent cells on each sample. Finally, the samples were turned
![Page 21: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/21.jpg)
20
upside down in a new 12-well plate and imaged using a Zeiss Axio Observer Z1 with
Zen 2 Pro Software.
2.5.3 Cell Adhesion and Proliferation Assays
To investigate with HCAECs, Mg-Zn alloy samples were placed individually into
12-well non-tissue culture plates and sterilized with UV light inside a biohazard hood
for one hour. 1 mL cell medium was added to each well and incubated for one hour.
Human Coronary Endothelial Cells were seeded onto each sample at a density of 10,
000 cells/ cm2. For cell adhesion, endothelial cells were incubated for 4 hours at 37 °C,
humidified 5% CO2 atmosphere. Cell proliferation was measured at 7 days and 14 days
of culture. Cell growth medium was changed every two days during proliferation period.
Phosphate-buffered saline (PBS) was used to wash off dead cells and 1 mL PBS was
added to each sample and aspirated before adding new growth medium. After the
incubation, each sample was washed with 1 mL PBS and an MTS dye (Promega)
solution at a 1:5 ratio (MTS: Medium) was prepared. Each sample was carefully
transferred to a new 12-well tissue culture plates with 1.2 mL MTS solution added into
![Page 22: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/22.jpg)
21
each well. Next, 12-well tissue culture plates were covered with aluminum foils and
cultured for another 4 hours to allow complete reaction of the MTS dye with the
metabolic products of the adherent cells. Then 100 μL of the reacted solution from each
well was transferred to a 96-well tissue culture plate in triplicate. Finally, cell density
data was determined from the absorbance measured by a plate reader (Molecular
Devices, SpectraMax M3) at 490 nm.
2.6 Statistics
All cell studies were conducted in triplicate and repeated at least two times. Data
were collected and the significant differences were assessed with the probability
associated with one way ANOVA tests only comparing with control data. Statistical
significance was considered at a p-value less than 0.05.
![Page 23: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/23.jpg)
22
3. RESULTS
3.1 Surface Characterization
ALD can be applied to any surface to allow titanium dioxide (TiO2) thin film
growth on top of flat or rough surfaces. It has been reported that crystal structures can
appear when TiO2 film growth temperature reaches above 165 °C 23. The surface
morphology of Mg-Zn alloy control and ALD-treated Mg-Zn alloy (150 °C and 200 °C)
was visualized by SEM (Figure 3A - 3C). It was clearly shown that TiO2 thin films
coated by ALD onto Mg-Zn alloy surfaces changed surface structures remarkably.
Agglomeration appeared intensively with an increase in temperature from 150 °C to
200 °C. Crystallites formed on the thin film surfaces can be observed with ALD
temperature at 200 °C. Since ALD can coat rough surfaces with all edges covered with
nanoscale thin film, the 100 nm TiO2 will be the first interface when interacting with
tissues in a biological environment. The elemental concentration of each SEM tested
sample was determined by EDAX as shown in the Appendix. In Table 1, summarized
elemental weight percentages and atomic percentages of TiO2 coated samples
compared with Mg-Zn alloy control. The notable increase of titanium (Ti) and oxygen
(O2) indicated the existence of TiO2 films deposited on the substrate surface.
![Page 24: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/24.jpg)
23
Table 1. Elemental concentrations of Mg-Zn alloy samples before and after ALD
by EDAX
Figure 3. SEM image of (A) Mg-Zn Control, (B) Mg-Zn-TiO2 (150°C), (C) Mg-
Zn-TiO2 (200°C); scale bars are 200nm
XPS graphs with titanium scans also showed the existence of TiO2 with two peaks
at 465 eV and 459 eV (Figure 4A). After 3 days of soaking in cell medium (Figure 4B),
TiO2 thin film layer disappeared since only one peak was presented for the sample with
a 200 °C ALD coating. TiO2 coated at 150 °C still presented two peaks (Figure 4B)
![Page 25: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/25.jpg)
24
indicating the maintenance of TiO2 thin film. The XRD patterns of tested samples are
shown in Figure 5. X-ray diffraction peaks were observed to fit with standard JCPDS
data and compared with similar Mg-Zn alloy patterns 24. A diffraction peak at 2θ=25.7 °
for Mg-Zn-TiO2 (200 °C) indicating the formation of TiO2 crystalline anatase while
comparing with Mg-Zn-TiO2 (150 °C) and control. Surface wettability, which is
determined by surface topography and chemistry, can further affect protein adsorption
on the surface of the substrate and therefore is one of the key factors for investigating
cell and bacteria activities at an interface between the implant and surrounding tissue
25,26. The surface wettability of Mg-Zn alloy control and Mg-Zn-TiO2 (150 °C and
200 °C) was determined from static water contact angle measurements. Hydrophobicity
and Hydrophilicity was determined by comparing contact angle results between
samples. In Figure 6, TiO2 coatings on Mg-Zn alloy substrates were found to be slightly
hydrophobic. Mg-Zn alloy control obtained a more hydrophilic property with contact
angles around 45 °. TiO2 coated at 150 °C showed a slight increase of contact angle
(~50 °) compared to control. The contact angle for 200 °C thin film coatings raised to
65° indicating that the sample is much more hydrophobic than the Mg-Zn control.
![Page 26: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/26.jpg)
25
Figure 4. XPS graphs for titanium scan of Mg-Zn alloy control and Mg-Zn-TiO2
coating at 150˚C and 200˚C; (A) without soak in medium (B) 3-day soak in
medium
Figure 5. XRD patterns of Mg-Zn alloy control and Mg-Zn-TiO2 coating at
150˚C and 200˚C
![Page 27: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/27.jpg)
26
Figure 6. Water contact angle measurements on Mg-Zn alloy samples with
different TiO2 ALD coatings temperatures. Data represents mean ± standard
deviation. **p<0.01; ***p<0.001 compared with control
3.2 Protein Adsorption Effect
According to the results obtained from BCA protein adsorption assay (Figure 7),
ALD-coated Mg-Zn alloy samples slightly increased protein adsorption when
compared with Mg-Zn control after the treatment in 0.01% BSA protein solution for 24
hours. The rising protein adsorption could be important for cell culture and bacteria
activities since proteins could interact with cell membranes and could protect surfaces
from being attacked by bacteria 27.
![Page 28: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/28.jpg)
27
Figure 7. The amount of adsorbed bovine serum albumin (BSA) protein on
sample surfaces after 24 hours of culture in a 0.01% BSA solution. Data
represents mean ± standard deviation.
3.3 Fluorescent Microscopy Assays
Fluorescent microscopy experiments employing Rhodamine/Hoechst (red/blue
signals) dyes were carried out. Fluorescent micrographs of HCAECs cultured for 4
hours on Mg-Zn control and Mg-Zn-TiO2 (150 °C and 200 °C) samples showed that
HCAECs will initially adhere on Mg-Zn alloy surfaces. Control samples clearly showed
cell adhesion on Mg-Zn with blue signals indicating cell cores stained by Rhodamine.
Red signals represent cell membranes stained by Hoechst dye. Live HCAECs before
cell fixation was represented by the overlay of red and blue signals. As shown in Figure
8A, without ALD coatings, HCAECs only adhered on sample surfaces but did not
![Page 29: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/29.jpg)
28
promote cell growth which corresponds to the reason why most of the live cells carried
out to have blue signals larger than red signals. Samples with TiO2 coated at 150 °C
showed impressive cell growth (Figure 8B) as majority of the cells were covered by red
signals rather than blue signals. The growth of cell membranes was indicated by the
spread of cell membranes (red signals) to represent the promotion of HCAECs under
fluorescent microscopes. On the other side, samples coated at 200 °C did not show
positive results correspond to cell adhesion and cell growth (Figure 8C).
![Page 30: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/30.jpg)
29
Figure 8. Fluorescent microscope image of (A) Mg-Zn Control, (B) Mg-Zn-TiO2
(150°C), (C) Mg-Zn-TiO2 (200°C)
![Page 31: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/31.jpg)
30
3.4 Cell Assays
Human Coronary Artery Endothelial Cells (HCAECs) form important cell
monolayer that lines blood vessels, maintains vascular tone, regulates hemostasis,
protects blood vessel from toxic matters, and controls inflammation 28. During PCI,
expanding of coronary stent might cause damage to the monolayer of HCAECs that
lines in the blood vessel. Therefore, a successful coronary scaffold should have the
ability to promote the growth of HCAECs in order to heal and reconstruct blood vessel.
In other words, a promising implantable material should accelerate HCAECs growth
and protect blood vessel that placed with coronary stents from inflammation, and
balance thrombosis and clotting. Thus, the effect of the nanoscale TiO2 thin film
coatings by ALD were investigated for Mg-Zn-TiO2 (150 °C and 200 °C) and Mg-Zn
control samples were chosen to investigate on HCAECs cell proliferation. As a result,
after 7 days and 14 days of cell culture, the endothelial cell density for Mg-Zn-TiO2
(150 °C) samples was enormously higher than those measured on Mg-Zn controls
(Figure 9). However, Mg-Zn-TiO2 (200 °C) samples did not show high promotion of
HCAECs and cell density. Unfortunately, the cell density decreased overtime when
comparing 7 days and 14 days of cell culture.
![Page 32: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/32.jpg)
31
Figure 9. Human coronary endothelial cell proliferation on Mg-Zn alloy control
and Mg-Zn-TiO2 (150 °C, 200 °C) samples. Data represents mean ± standard
deviation. **p<0.01; ***p<0.001 compared with control
![Page 33: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/33.jpg)
32
4. DISCUSSION
In this study, a well-established ALD coating technology with unique self-limiting
and self-terminating reaction characteristics was used to chemically graft TiO2 thin
coating with nanoscale thickness on the substrates of Mg-Zn binary alloy. ALD is a
more controllable coating method compare to other coating techniques such as CVD,
IBAD, and PLD for the deposition of uniform films with precise thickness. In addition,
the surface morphology of the deposited TiO2 film can be controlled by varying
processing temperature to achieve favorable crystallinity and surface structure 29.
Following the implantation of a material in the body, a series of biological events,
involving protein adsorption and cell adhesion, can occur on the surface of implanted
materials 30. Since the biomaterials are designed to function under physiological
environments, surface chemistry and topography of the materials are particularly
important for the advent of host responses and cell growth on the tissue-material
interface 31. Therefore, an ideal implant material should possess a biocompatible, non-
toxic and tolerable surface for higher tissue growth. Mg-Zn alloy is a conventional BVS
material that interacts with the coronary artery lumen. Therefore, Mg-Zn alloy was
selected to be modified with ALD treatment and investigated.
![Page 34: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/34.jpg)
33
Stenosis is caused by the deposition of excessive fat under endothelium. While
BVS is implanted into the coronary artery through PCI, a balloon is used to expand the
narrowed coronary artery for several times in order to reshape the bloodstream. As a
result, the diseased endothelium with excessive fat deposition beneath the vessel wall
is widened by the balloon and the blocked bloodstream is opened up. During the PCI
procedure, the sudden expansion and deployment of BVS can damage the endothelium
monolayer consisting of endothelial cells. The endothelium is the fundamental
regulator of vascular tone and thrombogenicity that separates blood stream components
such as platelets and the lumen wall 32. In particular, limited growth of HCAECs can
cause delayed revascularization process as well as in-stent inflammation and restenosis.
In our results, with the morphological observation by SEM images in Figure 3A –
3C, 100 nm TiO2 thin film can be clearly visualized comparing with untreated Mg-Zn
control. An intensive agglomeration with the raise of temperature was observed from
150 ˚C to 200 ˚C. Also, the SEM images in Figure 3 (C), TiO2 thin film coating at
200 °C showed higher distribution of visible crystallites compared to ALD coating at
150 °C (Figure 3B). The EDAX elemental composition analysis also indicated the
![Page 35: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/35.jpg)
34
existence of TiO2 thin film with increased elemental percentage of both Ti and O2
compared to control (Table 1). However, the different elemental percentage ratio of Ti
to O for ALD coating with the same thickness may be caused by the crystallite structure
formed by the TiO2 coating at 200 °C. TiO2 nano-thin film coating was reported to have
an unstable property with a coating temperature at 190 °C 19. XPS analysis also
illustrated the degradation of Mg-Zn-TiO2 (200 °C) after immersed in cell medium for
3 days (Figure 4B). The absence of the secondary TiO2 peak at 465eV in the XPS
spectra indicated degradation of the thin film. In contrast, the TiO2 thin film coating of
Mg-Zn-TiO2 (150 °C) remained stable after soaking in cell medium for 3 days. The
different surface crystallinity of Mg-Zn-TiO2 (200 °C) can be identified with the XRD
analysis. As shown in the XRD patterns (Figure 5), a peak representing TiO2 anatase
appeared at 2θ = 25.7 °, which was consistent as previously reported about the
formation of anatase crystallite on the surface of the material when TiO2 thin film was
deposited above 160 °C 33. Surface wettability showed Mg-Zn control to be more
hydrophilic (contact angle ~ 45 ˚) than ALD coated samples (Figure 6). TiO2 thin film
coated at 150 °C was slightly more hydrophobic (contact angle ~ 53 ˚) than control.
![Page 36: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/36.jpg)
35
Mg-Zn-TiO2 (200 °C) was the most hydrophobic sample among all the tested sample
with a contact angle around 65 ˚.
Furthermore, protein adsorption on the biomaterial surface is the initial event that
occurs when the BVS are implanted. The adsorbed protein layer can affect the
interactions of cells with the surface and allow for downstream cellular activities such
as cell adhesion and proliferation 34. Hydrophilicity of biomaterial surfaces is one of
the main factors that affect protein adsorption. Therefore, we measured the water
contact angles to evaluate the hydrophobicity of Mg-Zn substrates with or without ALD
treatment. The results showed that the ALD treatment caused the increase of water
contact angles, and thus, higher hydrophobicity. In addition, higher ALD operating
temperature resulted in an increase of water contact angle, suggesting that the
hydrophobicity of the ALD treated substrates could be altered with the operating
temperature. In the protein adsorption study, we used BSA as the model protein to
evaluated the level protein adsorption on the ALD treated Mg-Zn substrates. As Figure
7 shows, TiO2 nanoscale thin film grown on the Mg-Zn alloy substrates by ALD
(operated at 150 ˚C or 200 ˚C) showed a slight increase in BSA protein adsorption.
![Page 37: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/37.jpg)
36
Nonetheless, varying ALD operating temperatures did not induce significant
differences for protein adsorption results.
Next, we further analyzed HCAECs cell adhesion and cell proliferation on Mg-Zn
alloy substrates. The fluorescence micrographs (Figure 8) showed that HCAECs were
able to attach on the all the substrates in the first 4 h. The number of adhered cells on
Mg-TiO2-150 ˚C substrates was higher than those on control and Mg-TiO2-200 ˚C
substrates. Cells grown on Mg-TiO2-150 ˚C substrates also displayed greater cell
spreading and cytoskeleton development. The Mg-TiO2-200 °C samples showed
decreased cell number compared with the other two sample groups (Figure 8C).
However, after 7 days of cell culture, the binary alloy control and Mg-TiO2-200 ˚C
substrates induced very low HCAECs cell viability in vitro (Figure 9), and no
significant increase in cell density was observed after 14 days of cell culture. In contrast,
Mg-Zn-TiO2 (150 °C) samples resulted in pronounced proliferation of HCAECs over
7 days of cell culture with a cell density at 1.5x105 cells/cm2. After 14 days of cell
proliferation, HCAECs cell density grew even higher (2.0x105 cells/cm2). On the other
hand, Mg-Zn-TiO2 (200 °C) and Mg-Zn control samples did not promote cell growth.
![Page 38: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/38.jpg)
37
By looking at the results of 4-hour cell adhesion fluorescent images (Figure 8A),
although HCAECs adhered on the Mg-Zn control sample, cell cytoskeletons did not
spread to show any signs of cell growth. Mg-Zn-TiO2 (200 °C) induced similar cell
morphology but with less cell adhesion evidence (Figure 8C).
We hypothesized that ALD treatment with an operating temperature at 150 ˚C can
improve the biocompatibility of the Mg-Zn substrates to HCAECs. In contrary,
although cells could attach on the untreated substrates, cell proliferation was inhibited
by toxic substances generated by Mg degradation as a result of extended incubation
time. During Mg degradation, one of the side products, OH- ions, are generated. The
release of OH- ions may exhaust the physiological buffering system and cause further
tissue necrosis which results in cell death or changes in cell activities due to
alkalinization 35. This could be the reason for the low HCAECs viability on the
untreated Mg-Zn control. In addition, greater hydrophobicity of the Mg-Zn-TiO2 (200
˚C) samples with a different surface structure compared with Mg-Zn-TiO2 (150 ˚C) can
be unfavorable for cell growth, which showed a decreased in HCAECs density through
7-14 days of cell proliferation.
![Page 39: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/39.jpg)
38
Even though TiO2 thin film coated Mg-Zn alloy was slightly more hydrophobic
than the untreated substrates, the Mg-Zn-TiO2 (150 °C) sample promoted cell adhesion
and proliferation, indicating their potential to be a suitable BVS platform. On the other
hand, Mg-Zn-TiO2 (200 °C) with the same TiO2 thin film coating thickness (100 nm)
but different surface morphology was not suitable for implant materials since it is
unfavorable for cell adhesion and proliferation (Figure 8 and 9).
In summary, our study has shown that, with higher stability and biocompatibility,
TiO2 coated at 150 °C onto Mg-Zn alloy substrates showed promising potential to be
the bioresorbable materials for interventional cardiology applications such as BVS.
![Page 40: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/40.jpg)
39
5. CONCLUSION AND RECOMMENDATIONS
Using nano-thin film growth technology, ALD, to coat TiO2 on Mg-Zn alloy
substrates and served as BVS platform for the application of coronary artery
implantation showed promising endothelial cell adhesion and proliferation outcomes
with the temperature controlled at 150 °C. TiO2 nanoscale thin film acted as a protective
barrier prevented the substrates underneath the coating from interacting with
surrounding biological environments. In other words, the protective layer of TiO2 have
the potential to reduce the initial degradation rate of bare Mg-Zn alloy so that the
biomaterial will not loss its functionality before the completion of the revascularization
period (5-6 months). ALD coating at 200 °C did not show positive outcome with cell
assays due to its unstable surface morphology. Crystallites formed on the surface of the
coating changed its biocompatibility towards HCAECs and even killed cells. A well
designed fully bioresorbable implant material should promote endothelial cell growth
without additional drug elution. As a result, ALD thin film coating technology has a
strong potential to be applied to metallic coronary stent implant materials with an
optimized processing temperature control.
![Page 41: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/41.jpg)
40
As for future recommendations, long-term simulated body fluid (SBF) simulations
to obtain relatively reliable implant functioning period results in vitro would be
convincing to evaluate if the value meets the minimum revascularization requirement
(5-6 months). ALD TiO2 thin film coating can be further optimized to find the best
processing temperature for cell promotion. C-reactive protein (CRP) adsorption assays
testing ALD coating samples would be recommended since CRP is closely related to
in-stent inflammation responses which results in in-stent restenosis 36. It is also
recommended to conduct in vivo studies to further analyze the performance of this
technology.
![Page 42: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/42.jpg)
41
6. REFERENCES
1. Zipes, Douglas P., et al. “Braunwald's Heart Disease: a Textbook of Cardiovascular
Medicine.” Braunwald's Heart Disease: a Textbook of Cardiovascular Medicine, 2018.
2. Iqbal, Javaid, et al. “Coronary Stents: Historical Development, Current Status and Future
Directions.” British Medical Bulletin, vol. 106, no. 1, 2013, pp. 193–211.
3. Garg, Scot, and Patrick W. Serruys. “Coronary Stents Current Status.” Journal Of The
American College Of Cardiology, vol. 56, no. 10, 2010, pp. S1–S42.
4. Serruys, Pw, et al. “ANGIOGRAPHIC FOLLOW-UP AFTER PLACEMENT OF A
SELF-EXPANDING CORONARY-ARTERY STENT.” New England Journal Of
Medicine, vol. 324, no. 1, 1991, pp. 13–17.
5. Kereiakes, Dean J, et al. “Bioresorbable Vascular Scaffolds for Coronary
Revascularization.” Circulation, vol. 134, no. 2, 2016, pp. 168–82.
6. “Absorb Bioresorbable Vascular Scaffold System.” Home,
www.vascular.abbott/us/products/coronary-intervention/absorb-bioresorbable-
scaffold-dissolving-stent.html.
![Page 43: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/43.jpg)
42
7. Azzalini, Lorenzo, and Philippe L L'Allier. “Bioresorbable Vascular Scaffold
Thrombosis in an All-Comer Patient Population: Single-Center Experience.” The Journal
of Invasive Cardiology, vol. 27, no. 2, 2015, pp. 85–92.
8. “REal World Advanced Experience of BioResorbable ScaffolD by SMart Angioplasty
Research Team (SMART REWARD) - Full Text View.” Full Text View -
ClinicalTrials.gov, clinicaltrials.gov/ct2/show/NCT02601404.
9. Song, G., and Song, S. “A Possible Biodegradable Magnesium Implant Material.”
Advanced Engineering Materials, vol. 9, no. 4, 2007, pp. 298–302.
10. Li, Nan, and Yufeng Zheng. “Novel Magnesium Alloys Developed for Biomedical
Application: A Review.” Journal Of Materials Science &Amp; Technology, vol. 29, no. 6,
2013, pp. 489–502.
11. Tapiero, and Tew. “Trace Elements in Human Physiology and Pathology: Zinc and
Metallothioneins.” Biomedicine &Amp; Pharmacotherapy, vol. 57, no. 9, 2003, pp. 399–
411.
12. Bowen, Patrick K., et al. “Zinc Exhibits Ideal Physiological Corrosion Behavior for
Bioabsorbable Stents.” Advanced Materials, vol. 25, no. 18, 2013, pp. 2577–2582.
![Page 44: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/44.jpg)
43
13. Zhang, Shaoxiang, et al. “In Vitro Degradation, Hemolysis and MC3T3-E1 Cell
Adhesion of Biodegradable Mg–Zn Alloy.” Materials Science &Amp; Engineering C, vol.
29, no. 6, 2009, pp. 1907–1912.
14. Zhang, Shaoxiang, et al. “Research on an Mg–Zn Alloy as a Degradable Biomaterial.”
Acta Biomaterialia, vol. 6, no. 2, 2010, pp. 626–640.
15. Kirkland, N T. “Magnesium Biomaterials: Past, Present and Future.” Corrosion
Engineering, Science and Technology, vol. 47, no. 5, 2012, pp. 322–328.
16. Koch, C. F., et al. “Pulsed Laser Deposition of Hydroxyapatite Thin Films.” Materials
Science &Amp; Engineering C-Biomimetic And Supramolecular Systems, vol. 27, no. 3,
2007, pp. 484–494.
17. Yang, et al. “Modification of Degradation Behavior of Magnesium Alloy by IBAD
Coating of Calcium Phosphate.” Surface &Amp; Coatings Technology, vol. 202, no. 22,
2008, pp. 5733–5736.
18. Wank, Jeffrey R., et al. “Coating Fine Nickel Particles with Al 2 O 3 Utilizing an
Atomic Layer Deposition‐Fluidized Bed Reactor (ALD–FBR.” Journal of the American
Ceramic Society, vol. 87, no. 4, 2004, pp. 762–765.
![Page 45: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/45.jpg)
44
19. Liu L, et al. “Atomic Layer Deposition of Nano-TiO2 Thin Films with Enhanced
Biocompatibility and Antimicrobial Activity for Orthopedic Implants.” International
Journal of Nanomedicine, 2017, pp. 8711–8723.
20. Shen, G.X., et al. “Study on a Hydrophobic Nano-TiO2 Coating and Its Properties for
Corrosion Protection of Metals.” Electrochimica Acta, vol. 50, no. 25, 2005, pp. 5083–
5089.
21. Basiaga, Marcin, et al. “Influence of ALD Process Parameters on the Physical and
Chemical Properties of the Surface of Vascular Stents.” Archives of Civil and Mechanical
Engineering, vol. 17, no. 1, 2017, pp. 32–42.
22. Tzia Ming Onn, et al. “Atomic Layer Deposition on Porous Materials: Problems with
Conventional Approaches to Catalyst and Fuel Cell Electrode Preparation.” Inorganics, vol.
6, no. 1, 2018, pp.
23. Aarik, et al. “Morphology and Structure of TiO2 Thin Films Grown by Atomic Layer
Deposition.” Journal of Crystal Growth, vol. 148, no. 3, 1995, pp. 268–275.
![Page 46: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/46.jpg)
45
24. Jenei, et al. “X-Ray Diffraction Study on the Microstructure of a Mg–Zn–Y Alloy
Consolidated by High-Pressure Torsion.” Journal of Alloys and Compounds, vol. 539, no.
C, 2012, pp. 32–35.
25. Liu, Kesong, et al. “Bio-Inspired Titanium Dioxide Materials with Special Wettability
and Their Applications.” Chemical Reviews, vol. 114, no. 19, 2014, pp. 10044–10094.
26. Xu, and Siedlecki. “Effects of Surface Wettability and Contact Time on Protein
Adhesion to Biomaterial Surfaces.” Biomaterials, vol. 28, no. 22, 2007, pp. 3273–3283.
27. H.P. Felgueiras, J.C. Antunes, M.C.L. Martins, M.A. Barbosa,
“1 - Fundamentals of protein and cell interactions in biomaterials”, Editor(s): Mário A.
Barbosa, M. Cristina L. Martins, Peptides and Proteins as Biomaterials for Tissue
Regeneration and Repair, Woodhead Publishing, 2018, Pages 1-27.
28. Brutsaert, D L, et al. “Cardiac Endothelium and Myocardial Function.” Cardiovascular
Research, vol. 38, no. 2, 1998, pp. 281–90.
29. Miikkulainen, V, et al. “Crystallinity of Inorganic Films Grown by Atomic Layer
Deposition: Overview and General Trends.” Journal of Applied Physics, vol. 113, no. 2,
2013, pp.
![Page 47: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/47.jpg)
46
30. Rolfe, Barbara, et al. “The Fibrotic Response to Implanted Biomaterials:
Implications for Tissue Engineering.” Regenerative Medicine and Tissue Engineering
- Cells and Biomaterials, 2011, doi:10.5772/21790.
31. Chen, et al. “Biocompatible Polymer Materials: Role of Protein–Surface
Interactions.” Progress in Polymer Science, vol. 33, no. 11, 2008, pp. 1059–1087.
32. Sumpio, et al. “Cells in Focus: Endothelial Cell.” International Journal of Biochemistry
and Cell Biology, vol. 34, no. 12, 2002, pp. 1508–1512.
33. Luka, Grzegorz, et al. “Kinetics of Anatase Phase Formation in TiO2 Films during
Atomic Layer Deposition and Post-Deposition Annealing.” CrystEngComm, vol. 15, no.
46, 2013, pp. 9949–9954.
34. Anderson, Jm. “Biological Responses to Materials.” Annual Review Of Materials
Research, vol. 31, 2001, pp. 81–110.
35. Seitz, J.‐M., et al. “Magnesium Degradation Products: Effects on Tissue and Human
Metabolism.” Journal of Biomedical Materials Research Part A, vol. 102, no. 10, 2014,
pp. 3744–3753.
![Page 48: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/48.jpg)
47
36. Li, Jian-Jun, et al. “Impact of C-Reactive Protein on in-Stent Restenosis: a Meta-
Analysis.” Texas Heart Institute Journal, vol. 37, no. 1, 2010, pp. 49–57.
7. APPENDIX
Figure 9. EDAX data results for Mg-Zn alloy control
![Page 49: Atomic Layer Deposition Coating Titanium Dioxide Nano-thin ...m044c3844/... · Atomic Layer Deposition Coating Titanium Dioxide Nano-thin Film on Magnesium-Zinc Alloy to Enhance Cytocompatibility](https://reader033.fdocuments.net/reader033/viewer/2022052007/601bbfc4461f686430690125/html5/thumbnails/49.jpg)
48
Figure 10. EDAX data results for Mg-Zn-TiO2-150 ˚C
Figure 11. EDAX data results for Mg-Zn-TiO2-200 ˚C