3 concrete structures defects 2
Transcript of 3 concrete structures defects 2
![Page 1: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/1.jpg)
Base - Isolation
![Page 2: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/2.jpg)
![Page 3: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/3.jpg)
Base Isolators
![Page 4: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/4.jpg)
3- Earthquake Hinge
4
![Page 5: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/5.jpg)
Earthquake Hinge
5
![Page 6: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/6.jpg)
6
Carbon-fiber-reinforced polymer or
carbon-fiber-reinforced plastic
(CFRP or CRP)
![Page 7: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/7.jpg)
Typical Properties High StrengthHigh
ModulusUltra-High Modulus
Density (g/cm3) 1.8 1.9 2.0 - 2.1
Young's Modulus (GPa) 230 370 520 - 620
Tensile Strength (GPa) 2.48 1.79 1.03 - 1.31
Tensile Elongation (%) 1.1 0.5 0.2
Table for carbon fibers
![Page 8: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/8.jpg)
8
![Page 9: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/9.jpg)
9
![Page 10: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/10.jpg)
10
FRP Sheet
FRP Plate
![Page 11: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/11.jpg)
• FRP can be applied to strengthen:
1. Beams
2. Columns
3. Slabs of buildings and bridges
• It is possible to increase the strength of structuralmembers even after they have been severelydamaged due to loading conditions. In the case ofdamaged reinforced concrete members:
1. Repairing of the member by removing loose debrisand filling in cavities and cracks with mortar orepoxy resin.
2. Strengthening through the fibre sheets with epoxyresin then applying them to the cleaned andprepared surfaces of the member.
11
![Page 12: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/12.jpg)
Two techniques are typically adopted for thestrengthening of beams, relating to the strengthenhancement desired:
– Flexural strengthening
– Shear strengthening
• For the flexural strengthening of a beam,
FRP sheets or plates are applied to the tensionface of the member.
Principal tensile fibers are oriented in the beamlongitudinal axis, similar to its internal flexuralsteel reinforcement. This increases the beamstrength and deflection capacity, and its stiffness(load required to cause unit deflection).
12
Beams
![Page 13: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/13.jpg)
flexural strengthening of a beam
13
![Page 14: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/14.jpg)
• For the shear strengthening of a beam, the FRP is applied on the web orside faces of the member with fibers oriented transverse to the beamlongitudinal axis.
• This is necessary for resisting shear forces, in a similar manner as internalsteel stirrups, by bridging shear cracks that form under loading andrestricting their growth.
• The FRP can be applied in several configurations, this includes:1. Side bonding2. U-wraps or U-jackets3. Closed wraps or complete wraps.• Side bonding involves applying FRP to both sides of the beam only. It
provides the least amount of shear strengthening due to failures causedby debonding of the FRP from the concrete surface at the free edges.
• U-wraps, for which the FRP is applied continuously in a 'U' shape aroundthe sides and bottom (tension) face of the beam.
• closed wraps, If all faces of a beam are accessible, then the use of closedwraps is desirable to provide the most strength enhancement. Closedwrapping involves applying FRP around the entire perimeter of themember with an overlap of FRP.
• For all wrap configurations, the FRP can be applied along the length ofthe member as a continuous sheet or as discrete strips, having apredefined minimum width and spacing.
14
![Page 15: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/15.jpg)
Shear strengthening of a beam
15
FRP is applied continuously
Side bonding involves applying FRP to both sides of the beam only
![Page 16: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/16.jpg)
Carbon-fiber-reinforced polymer or carbon-fiber-reinforced plastic (CFRP or CRP or often simply carbon fiber)
Structural Defects – strengthening U-wraps or U-jackets
16
![Page 17: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/17.jpg)
Flexural and shear (U-wraps or U-jackets)strengthening of a beam
17
![Page 18: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/18.jpg)
Flexural and shear strengthening of a beam
18
![Page 19: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/19.jpg)
Flexural and shear strengthening of a beamaccording to bending moment diagram
19
![Page 20: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/20.jpg)
flexural strengthening of a beam
20
![Page 21: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/21.jpg)
21Shear strengthening of a beam, FRP is applied continuously
U-wraps or U-jackets
![Page 22: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/22.jpg)
• Slabs may be strengthened by applying FRP strips at theirbottom (tension) face. This will result in better flexuralperformance, since the tensile resistance of the slabs issupplemented by the tensile strength of FRP. In the case ofbeams and slabs, the effectiveness of FRP strengtheningdepends on the performance of the resin chosen forbonding. This is particularly an issue for shear strengtheningusing side bonding or U-wraps.
22
Slabs of buildings and bridges
![Page 23: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/23.jpg)
23
Slab opening
Anchorage for slab ConcreteRetrofitting
![Page 24: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/24.jpg)
24
![Page 25: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/25.jpg)
• Columns are typically wrapped with FRParound their perimeter, as with closed orcomplete wrapping. This not only results inhigher shear resistance, but more crucial forcolumn design, it results in increasedcompressive strength under axial loading.The FRP wrap works by:
25
Restraining the lateral expansion of thecolumn, which can enhance confinement in asimilar manner as spiral reinforcement doesfor the column core.
![Page 26: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/26.jpg)
Closed wraps or complete wraps for columns
26
Columns are typically wrapped with FRP
![Page 27: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/27.jpg)
Closed wraps for columns
27
![Page 28: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/28.jpg)
Closed wraps for columns and shear strengthening of a beam
28
![Page 29: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/29.jpg)
5- Leakage of water
29
![Page 30: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/30.jpg)
Leakage of water
30
![Page 31: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/31.jpg)
Leakage of water
31
![Page 32: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/32.jpg)
6- Collapse
32
![Page 33: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/33.jpg)
Collapse
33
![Page 34: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/34.jpg)
Collapse
34
![Page 35: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/35.jpg)
Collapse
35
![Page 36: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/36.jpg)
Collapse
36
![Page 37: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/37.jpg)
Collapse
37
![Page 38: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/38.jpg)
Collapse
38
![Page 39: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/39.jpg)
7- Corrosion of reinforcement
Corrosion: Corrosion of reinforcing steel and other embedded metals is one of the leading causes of deterioration of concrete. When steel corrodes, the resulting rust occupies a greater volume than steel. The expansion creates tensile stresses in the concrete, which can eventually cause cracking and spalling.
39
![Page 40: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/40.jpg)
Corrosion of Steel Reinforcement
40
![Page 41: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/41.jpg)
Corrosion of Steel Reinforcement
41
![Page 42: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/42.jpg)
Corrosion of Steel Reinforcement
42
![Page 43: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/43.jpg)
Corrosion of Steel Reinforcement
43
![Page 44: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/44.jpg)
@Corrosion of Steel Reinforcement
44
![Page 45: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/45.jpg)
Corrosion of Steel Reinforcement
45
![Page 46: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/46.jpg)
Corrosion of Steel Reinforcement
46
![Page 47: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/47.jpg)
Column corner corrosion
47
![Page 48: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/48.jpg)
Mode of failure and corrosion
48
![Page 49: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/49.jpg)
Corrosion of reinforcement- Corrosion of steel reinforcement bar is anelectrochemical process that requires:
1- Oxidizing agent.
2- Moisture.
3- Electron flow.
The key to protecting steel from corrosion is to stop or reverse the chemicalreactions. This may be done by cutting off the supplies of oxygen ormoisture or by supplying excess electrons at the anodes to prevent theformation of the metal ions (cathodic protection). Cracks provide easyaccess for oxygen, moisture, and chlorides, and thus, minor splittingcracks can create a condition in which corrosion and cracking areaccelerated. The protection against corrosion-induced:
1. Use of concrete with low permeability.
2. Adequate cover.
3. In very severe exposure conditions, coated reinforcement.
4. Sealers or overlays on the concrete.
5. Corrosion-inhibiting admixtures.
6. Cathodic protection. 49
Mechanism of steel reinforcement corrosion
![Page 50: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/50.jpg)
Anodic reaction Fe2 2Fe2+ +2e-
Cathodic reaction 4e- + O2 + 2H2O 4(OH)-
2Fe2+ +2 OH- Fe(OH)2 Ferrous hydroxide4 Fe(OH)2 + 2H2O + O2 4Fe(OH)3 Ferric Hydroxide
Normalmechanism of corrosion
Anode Cathode
Fe++ 2e-
2OH _Fe (OH)2
H2O + ½ O2
Ph. less than 10.5
Mechanism of steel reinforcement corrosion
![Page 51: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/51.jpg)
passive film by Kerber el at.(1990):Hydrated Ferric oxide or Ferric oxide
passive film by Hanson at.(1984):Inner layer: Ferrous Oxide .Outer layer : Ferric Oxide
Concrete cover (PH value =12-13)
Marine Environment
Chloride Ions
Corrosion product ferrous hydroxide
Concrete cover (PH value =8-9(through carbonation)
Steel corrosion in marine environment concrete
![Page 52: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/52.jpg)
52
The corrosion of steel reinforced concrete member by the formation of electro-chemical cell results in cracking (characteristically parallel to the reinforcement), spalling or in delamination of concrete. This corrosion may occur due to chloride attack and carbonation.
Cases of steel corrosion in slabs
Delamination
![Page 53: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/53.jpg)
53Sacrificial anode system in seawater
![Page 54: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/54.jpg)
54Impressed-current cathodic-protection system in seawater
Supplying excess electrons at the anodes to prevent the formation of the metal ions (cathodic protection).
![Page 55: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/55.jpg)
Improper casting
55
![Page 56: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/56.jpg)
Inadequate Concrete Cover
56
![Page 57: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/57.jpg)
8- Settlement of the foundation
57
![Page 58: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/58.jpg)
Settlement of the foundation
58
![Page 59: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/59.jpg)
Settlement of the foundation
59
![Page 60: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/60.jpg)
• What Causes A Concrete Floor Slab To Settle?• When a concrete floor settles, it can mean
serious damage. The causes of floor slab settlement are almost always due to the soils underneath being unable to support the weight of the concrete.
• The three most common causes of settling concrete floor slabs are as follows:
1- Drying/Shrinking Of Soils Under The Slab. 2- Washout Of Soil Underneath The Slab.3- Poor Compaction Of Foundation Fill Soils.
60
Settlement
![Page 61: 3 concrete structures defects 2](https://reader031.fdocuments.net/reader031/viewer/2022022413/58f00b411a28ab6b608b468b/html5/thumbnails/61.jpg)
Causes of Settlement
61
Drying/Shrinking Of Soils Under The Slab
Washout Of Soil Underneath The Slab
Poor Compaction Of Foundation Fill Soils