28119167 Corrosion of Superalloys[1]
Transcript of 28119167 Corrosion of Superalloys[1]
![Page 1: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/1.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 1/36
![Page 2: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/2.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 2/36
![Page 3: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/3.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 3/36
![Page 4: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/4.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 4/36
![Page 5: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/5.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 5/36
![Page 6: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/6.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 6/36
![Page 7: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/7.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 7/36
![Page 8: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/8.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 8/36
![Page 9: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/9.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 9/36
![Page 10: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/10.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 10/36
![Page 11: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/11.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 11/36
![Page 12: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/12.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 12/36
![Page 13: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/13.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 13/36
![Page 14: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/14.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 14/36
![Page 15: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/15.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 15/36
![Page 16: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/16.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 16/36
![Page 17: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/17.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 17/36
![Page 18: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/18.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 18/36
![Page 19: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/19.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 19/36
![Page 20: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/20.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 20/36
![Page 21: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/21.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 21/36
![Page 22: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/22.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 22/36
![Page 23: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/23.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 23/36
![Page 24: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/24.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 24/36
![Page 25: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/25.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 25/36
![Page 26: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/26.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 26/36
![Page 27: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/27.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 27/36
![Page 28: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/28.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 28/36
![Page 29: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/29.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 29/36
![Page 30: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/30.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 30/36
![Page 31: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/31.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 31/36
![Page 32: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/32.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 32/36
![Page 33: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/33.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 33/36
![Page 34: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/34.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 34/36
![Page 35: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/35.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 35/36
![Page 36: 28119167 Corrosion of Superalloys[1]](https://reader033.fdocuments.net/reader033/viewer/2022051009/577d2ae91a28ab4e1eaa6cd2/html5/thumbnails/36.jpg)
8/7/2019 28119167 Corrosion of Superalloys[1]
http://slidepdf.com/reader/full/28119167-corrosion-of-superalloys1 36/36